Formula of novel logistics tray
A pallet and logistics technology, which is applied in the formulation field of new logistics pallets, can solve the problem of low surface energy, achieve the effects of improving surface energy, avoiding poor cementation effect, and facilitating automatic implementation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A formula for a novel logistics tray, the logistics tray is made up of the following components, 88.2% PP (polypropylene), 2.0% HDPE (hot-melt resin), 0.10% defoamer, 5.0% POE (thermoplastic elastic Body), 1.8% color masterbatch and 2.46% 30% sodium hydroxide solution and 0.10% degreasing mixed solution.
[0023] Among them, the specific process is as follows:
[0024] Step 1, sieving and proportioning, firstly sieve each component, and then carry out proportioning and weighing of each sieved component.
[0025] Step 2, mixing and stirring, put the raw materials weighed in proportion into the deceleration mixer, stir and mix, and during the stirring process, heat the inside of the high-speed mixer, after heating to 300 degrees, the sodium hydroxide solution and the chromium 10% acid; 60% water; a mixed solution composed of 30% concentrated sulfuric acid, and under the action of the corresponding rotating speed, the components are mixed evenly and fully to obtain a mixt...
Embodiment 2
[0034] 88.2% PP (polypropylene), 5.0% HDPE (hot melt resin), 0.30% defoamer, 0.1% POE (thermoplastic elastomer), 1.8% color masterbatch and 3.0% 30% sodium hydroxide solution and a 1.6% degreasing mixed solution.
[0035] Among them, the specific process is as follows:
[0036] Step 1, sieving and proportioning, firstly sieve each component, and then carry out proportioning and weighing of each sieved component.
[0037] Step 2, mixing and stirring, put the raw materials weighed in proportion into the deceleration mixer, stir and mix, and during the stirring process, heat the inside of the high-speed mixer, after heating to 300 degrees, the sodium hydroxide solution and the chromium 10% acid; 60% water; a mixed solution composed of 30% concentrated sulfuric acid, and under the action of the corresponding rotating speed, the components are mixed evenly and fully to obtain a mixture;
[0038] Step 3, the mixture is left to stand, and the mixture is left to stand for 3 hours, t...
Embodiment 3
[0046] 88.2% PP (polypropylene), 4.0% HDPE (hot melt resin), 0.30% defoamer, 0.1% POE (thermoplastic elastomer), 1.8% color masterbatch and 2.0% 30% sodium hydroxide solution and a 3.6% degreasing mixed solution.
[0047] Among them, the specific process is as follows:
[0048] Step 1, sieving and proportioning, firstly sieve each component, and then carry out proportioning and weighing of each sieved component.
[0049] Step 2, mixing and stirring, put the raw materials weighed in proportion into the deceleration mixer, stir and mix, and during the stirring process, heat the inside of the high-speed mixer, after heating to 300 degrees, the sodium hydroxide solution and the chromium 10% acid; 60% water; a mixed solution composed of 30% concentrated sulfuric acid, and under the action of the corresponding rotating speed, the components are mixed evenly and fully to obtain a mixture;
[0050] Step 3, the mixture is left to stand, and the mixture is left to stand for 3 hours, t...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com