Preparation method and application of magnetic Co-V/C3N3 composite supporter particles
A composite carrier, C3N3 technology, applied in the field of water treatment, can solve the problems of large-scale development and application of unfavorable technologies, low-refractory organic wastewater treatment, unstable transportation, storage, etc., and achieve low cost, low equipment requirements, and convenient operation Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] Among them, magnetic Co-V / C 3 N 3 Composite carrier particles are prepared by the following methods:
[0028] Step 1: 0.8g of Co(NO 3 ) 3 Dissolve in 5ml of deionized water, add 100ml of absolute ethanol, and mix evenly to obtain solution A; commercial C 3 N 4 Grind into powder and add to solution A. After continuous stirring, place the mixed solution in ultrasonic treatment for 40 minutes, then dry it at 105°C for 10 hours, and put the obtained solid substance in a muffle furnace for roasting at 500°C. 3h, get Co / C 3 N 4 Carrier particles;
[0029] Step 2: Dissolve 0.5g of ammonium metavanadate in 5ml of deionized water (stir to make it dissolve completely and then add a phosphoric acid solution with a mass fraction of 80%, and the phosphoric acid solution in every 5ml of solution is 0.1g to 0.2g to obtain solution B , the Co / C obtained in step 1 3 N 4 Carrier particles were added to solution B, and then ultrasonically treated for 30 minutes after continuous st...
Embodiment 2
[0033] Among them, magnetic Co-V / C 3 N 3 Composite carrier particles are prepared by the following methods:
[0034] Step 1: 0.5g of Co(NO 3 ) 3 Dissolve in 5ml of deionized water, add 100ml of absolute ethanol, and mix evenly to obtain solution A; commercial C 3 N 4 Grind into powder and add to solution A. After continuous stirring, place the mixed solution in ultrasonic treatment for 50 minutes, then dry at 105°C for 11 hours, and place the obtained solid substance in a muffle furnace for 4 hours at 500°C. , get Co / C 3 N 4 Carrier particles;
[0035] Step 2: Dissolve 0.6g of ammonium metavanadate in 5ml of deionized water (stir to make it dissolve completely and then add a phosphoric acid solution with a mass fraction of 80%, and the phosphoric acid solution in every 5ml of solution is 0.1g to 0.2g to obtain solution B , the Co / C obtained in step 1 3 N 4 Carrier particles were added to solution B, and then ultrasonically treated for 40 minutes after continuous stir...
PUM
Property | Measurement | Unit |
---|---|---|
particle size (mesh) | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com