Embodiment 1
[0022] The washing method of pseudo-boehmite comprises the following steps:
[0023] S1 First washing: After filtering the aged pseudo-boehmite slurry, the filter residue is discharged into the primary washing tank, and mixed with the secondary filtrate sent from the secondary washing liquid storage tank to complete the first washing. The volume ratio is 15:1, and the mixing time is 40 minutes;
[0024] S2 second washing: after the first washing, filter again, the primary filtrate flows into the primary washing liquid storage tank, and the primary filter residue is discharged into the secondary washing tank, and mixed with the four filtrates sent from the fourth washing liquid storage tank to complete For the second washing, the liquid-solid volume ratio is 20:1, and the mixing time is 30 minutes;
[0025] S3 third washing: after the second washing, filter again, the secondary filtrate flows into the secondary washing liquid storage tank and then pumps it into the primary was...
Embodiment 2
[0030] The washing method of pseudo-boehmite comprises the following steps:
[0031] S1 First washing: After filtering the aged pseudo-boehmite slurry, the filter residue is discharged into the primary washing tank, and mixed with the secondary filtrate sent from the secondary washing liquid storage tank to complete the first washing. The volume ratio is 20:1, and the mixing time is 20 minutes;
[0032] S2 second washing: after the first washing, filter again, the primary filtrate flows into the primary washing liquid storage tank, and the primary filter residue is discharged into the secondary washing tank, and mixed with the four filtrates sent from the fourth washing liquid storage tank to complete For the second washing, the liquid-solid volume ratio is 20:1, and the mixing time is 40 minutes;
[0033] S3 third washing: after the second washing, filter again, the secondary filtrate flows into the secondary washing liquid storage tank and then pumps it into the primary was...
Embodiment 3
[0038] The washing method of pseudo-boehmite comprises the following steps:
[0039] S1 First washing: After filtering the aged pseudo-boehmite slurry, the filter residue is discharged into the primary washing tank, stirred and mixed with the secondary filtrate sent from the secondary washing liquid storage tank, and heated to 50°C with steam Complete the first washing, the liquid-solid volume ratio is 20:1, and the mixing time is 20 minutes;
[0040] S2 Second washing: After the first washing, filter again, the primary filtrate flows into the primary washing liquid storage tank, and the primary filter residue is discharged into the secondary washing tank, mixed with the fourth filtrate from the fourth washing liquid storage tank and passed through Put in steam and heat to 50°C and stir to complete the second washing, the liquid-solid volume ratio is 20:1, and the stirring and mixing time is 40 minutes;
[0041] S3 third washing: after the second washing, filter again, the se...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com