A friction-resistant, alumina technology, applied in the preparation and coating of aluminum hydroxide, can solve the problems of poor friction resistance of organic films, large amount of sol in the pulling method, and high price of aluminum isopropoxide, so as to avoid large areas. The effect of corrosion, shortening the production time, and controlling the degree of corrosion
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] The method for making aluminum hydroxide sol from aluminum sec-butoxide comprises the following steps:
[0025] 1) Preparation of alumina sol: 24.6 g of aluminum sec-butoxide was added to 180 g of distilled water at 85°C, stirred with magnetic force for 30 minutes, adjusted to pH 2 with 6 ml of nitric acid, and magnetically stirred at 85°C for 30 minutes to obtain alumina sol, The sol is aged for 5 days for use;
[0026] 2) Preparation of the glass carrier: take the slides and wash them in a sonicator with 100 ml of ethyl acetate, 100 ml of 95% ethanol, and 100 ml of deionized water in sequence for 30 minutes, and dry them for use;
[0027] 3) Repeated coating: Coat the glass carrier by spray method, dry it at room temperature for 1 day, and sinter it with a muffle furnace. The initial temperature is set to 50 °C, the heating rate is 1 °C / min, the temperature is kept at 200 °C for 30 minutes, and the temperature is kept at 350 °C. 30min, hold at 550℃ for 3h, repeat the...
Embodiment 2
[0031] The method for making aluminum hydroxide sol from aluminum sec-butoxide comprises the following steps:
[0032] 1) Preparation of alumina sol: 49.2 g of aluminum sec-butoxide was added to 360 g of distilled water at 85°C, stirred with magnetic force for 30min, adjusted to pH 2 with 12ml of nitric acid, and magnetically stirred at 85°C for 30min to obtain alumina sol, The sol is aged for 5 days for use;
[0033] 2) Preparation of the glass carrier: take the slides and wash them in a sonicator with 100 ml of ethyl acetate, 100 ml of 95% ethanol, and 100 ml of deionized water in sequence for 30 minutes, and dry them for use;
[0034] 3) Repeated coating: Coat the glass carrier by spray method, dry it at room temperature for 1 day, and sinter it with a muffle furnace. The initial temperature is set to 50 °C, the heating rate is 1 °C / min, the temperature is kept at 200 °C for 30 minutes, and the temperature is kept at 350 °C. 30min, hold at 550℃ for 1h, repeat the coating f...
Embodiment 3
[0038] The method for making aluminum hydroxide sol from aluminum sec-butoxide comprises the following steps:
[0039] 1) Preparation of alumina sol: 147.8 g of aluminum sec-butoxide was added to 1080 g of distilled water at 85°C, stirred with magnetic force for 30min, adjusted to pH 2 with 18ml of nitric acid, and magnetically stirred at 85°C for 30min to obtain alumina sol, The sol is aged for 5 days for use;
[0040] 2) Preparation of the glass carrier: take the slides and wash them in a sonicator with 100 ml of ethyl acetate, 100 ml of 95% ethanol, and 100 ml of deionized water in sequence for 30 minutes, and dry them for use;
[0041] 3) Repeated coating: Coat the glass carrier by spray method, dry it at room temperature for 1 day, and sinter it with a muffle furnace. The initial temperature is set to 50 °C, the heating rate is 1 °C / min, the temperature is kept at 200 °C for 30 minutes, and the temperature is kept at 350 °C. 30min, hold at 550℃ for 3h, repeat the coating...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com