Embodiment 1
[0018] Include the following steps:
[0019] (1) Decomposition of remaining cyanide in cyanide slag:
[0020] The cyanide slag is prepared into a slurry with a concentration of 30%, and the remaining cyanide in the slurry is treated by Colt’s acid method;
[0021] (2) Slurry flotation pyrite operation after Colt’s acid treatment includes:
[0022] (a) Add the ore pulp that step (1) obtains into the flotation machine; Add H 2 SO 4 Make the pH value of the pulp reach 4, then add 525g / t sodium polyphosphate, 525g / t sodium fluorosilicate as regulator, 110g / t butyl xanthate as collector, 42.5g / t methyl isobutyl carbinol As a foaming agent, the first roughing operation is carried out to obtain the first roughing concentrate;
[0023] (b) Add 525g / t sodium polyphosphate and 525g / t sodium fluorosilicate to the pulp in step (a) as regulator, 110g / t butyl xanthate as collector, 42.5g / t methyl isobutyl Base methanol is used as a foaming agent to carry out the second roughing operati...
Embodiment 2
[0027] Include the following steps:
[0028] (1) Decomposition of remaining cyanide in cyanide slag:
[0029] The cyanide slag is prepared into a slurry with a concentration of 30%, and the remaining cyanide in the slurry is treated by Colt’s acid method;
[0030] (2) Slurry flotation pyrite operation after Colt’s acid treatment includes:
[0031] (a) Add the ore pulp that step (1) obtains into the flotation machine; Add H 2 SO 4 Make the pH value of the pulp reach 4, then add 500g / t sodium polyphosphate, 500g / t sodium fluorosilicate as regulator, 100g / t butyl xanthate as collector, 40g / t methyl isobutyl carbinol as The foaming agent is used for the first roughing operation to obtain the first roughing concentrate;
[0032] (b) Add 500g / t sodium polyphosphate, 500g / t sodium fluorosilicate to the pulp in step (a) as regulator, 100g / t butyl xanthate as collector, 40g / t methyl isobutyl Methanol is used as a foaming agent to carry out the second roughing operation to obtain t...
Embodiment 3
[0036] Include the following steps:
[0037] (1) Decomposition of remaining cyanide in cyanide slag:
[0038] The cyanide slag is prepared into a slurry with a concentration of 30%, and the remaining cyanide in the slurry is treated by Colt’s acid method;
[0039] (2) Slurry flotation pyrite operation after Colt’s acid treatment includes:
[0040] (a) Add the ore pulp that step (1) obtains into the flotation machine; Add H 2 SO 4 Make the pH value of the pulp reach 4, then add 550g / t sodium polyphosphate, 550g / t sodium fluorosilicate as regulator, 120g / t butyl xanthate as collector, 45g / t methyl isobutyl carbinol as The foaming agent is used for the first roughing operation to obtain the first roughing concentrate;
[0041] (b) Add 550g / t sodium polyphosphate, 550g / t sodium fluorosilicate to the pulp in step (a) as regulator, 120g / t butyl xanthate as collector, 45g / t methyl isobutyl Methanol is used as a foaming agent to carry out the second roughing operation to obtain t...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
boiling point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com