Method for increasing extraction rate of mid-low-grade phosphate rock
A low-grade, extraction-rate technology, applied in chemical instruments and methods, phosphorus compounds, phosphate material treatment, etc., can solve problems such as waste of resources, achieve the effects of saving resources, preventing flocculation, and solving difficult utilization
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Put the low-grade phosphate rock with a content of 25.4% into the crusher for coarse crushing first, and the coarsely crushed phosphate rock will directly enter the ball mill. At the same time, add water and dispersant to the ball mill to grind the phosphate rock into pulp. Pour it into the extraction tank and extract it with sulfuric acid to obtain phosphoric acid.
[0021] The mass ratio of phosphate rock, water, hydrolyzed polymaleic anhydride, sodium polyacrylate, 5040 dispersant and sulfuric acid is: 40:17:0.6:0.4:0.3:41.7.
[0022] The extraction rate of phosphate rock was detected to be 98.2%.
Embodiment 2
[0024] Put the low-grade phosphate rock with a content of 25.4% into the crusher for coarse crushing first, and the coarsely crushed phosphate rock will directly enter the ball mill. At the same time, add water and dispersant to the ball mill to grind the phosphate rock into pulp. Pour it into the extraction tank and extract it with sulfuric acid to obtain phosphoric acid.
[0025] The mass ratio of phosphate rock, water, hydrolyzed polymaleic anhydride, sodium polyacrylate, 5040 dispersant and sulfuric acid is: 40:17:0.6:0.4:42.
[0026] The extraction rate of phosphate rock was detected to be 98.6%.
Embodiment 3
[0028] Put the low-grade phosphate rock with a content of 25.4% into the crusher for coarse crushing first, and the coarsely crushed phosphate rock will directly enter the ball mill. At the same time, add water and dispersant to the ball mill to grind the phosphate rock into pulp. Pour it into the extraction tank and extract it with sulfuric acid to obtain phosphoric acid.
[0029] The mass ratio of phosphate rock, water, hydrolyzed polymaleic anhydride, sodium polyacrylate and sulfuric acid is: 40:17:0.4:0.6:42.
[0030] The extraction rate of phosphate rock was detected to be 97.8%.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com