Glue, and plastic and metal composite housing preparation method
A glue and water-based technology, applied in the direction of adhesives, rosin adhesives, etc., can solve problems such as cleaning, product approval, and damage to molds
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0037] The present invention also provides a method for preparing a plastic and metal composite shell, the method comprising the following steps:
[0038] S1. Coating glue on the metal surface to be combined with plastic, and then surface-drying the glue;
[0039] S2. Put the metal obtained in step S1 into a mold to inject plastic to obtain an assembly;
[0040] S3, baking the assembly;
[0041] S4, performing anodic oxidation on the baked assembly to obtain a plastic and metal composite shell;
[0042] Wherein, the glue is the glue described in the present invention.
[0043] In the present invention, the glue that can be cross-linked twice is coated on the joint position of the metal and plastic integrated product, so that the assembly becomes an absolutely integrated product (there is no gap at the joint of the composition, that is, the glue combines with the metal and plastic and penetrates into the joint. In the two interfaces), so as to prevent this type of assembly p...
Embodiment 1
[0051] 1. Prepare glue
[0052] (1) Take the experimental cup 1 and introduce 40g of water-based self-crosslinking acrylic resin Geely-832 (TG value: 65°C) into the experimental container. Then add 20g of water-based rosin tackifying resin and stir evenly with a glass rod. Add 0.1g of additive glide-410 to increase fluidity. Then add 0.1 g of defoamer BYK-020. Then add 0.3g adhesion promoter Dow Corning-6040. Add 10g of n-butanol, and then stir evenly with a glass rod for 5 minutes to better disperse the leveling agent, defoamer, and accelerator.
[0053] (2) Finally, add 6.5g of deionized water to adjust the viscosity, and stir evenly for 5 minutes. Stand still for 20 minutes to allow the air bubbles during stirring to dissipate to obtain component A1.
[0054] (3) Take another experimental cup 2 and add 15g of polyamide particles. Then add 8g of PA treatment agent, stir for 10 minutes, and stand still for 10 minutes to obtain component B1.
[0055] (4) Mix component B...
Embodiment 2
[0063] 1. Prepare glue
[0064] (1) Take the experimental cup 1 and introduce 60g of water-based self-crosslinking acrylic resin Geely-832 into the experimental container. Then add 10g of water-based rosin tackifying resin and stir evenly with a glass rod. Add 0.21g of additive glide-410 to increase fluidity. Then add 0.2 g of defoamer BYK-020. Then add 0.5g adhesion promoter Dow Corning-6040. Add 7g of the first solvent n-butanol, and then stir evenly with a glass rod for 3 minutes to better disperse the leveling agent, defoamer, and accelerator.
[0065] (2) Finally, add 3g of deionized water to adjust the viscosity, and stir evenly for 5 minutes. Stand still for 20 minutes to allow the air bubbles during stirring to dissipate to obtain component A2.
[0066] (3) Take another test cup 2 and add 10g of polyamide particles. Then add 9.7g of polyamide treatment agent, stir for 10 minutes, and stand still for 10 minutes to obtain component B2.
[0067] (4) Mix component B...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com