Embodiment 1
[0018] Embodiment one: a kind of super early strength agent of Portland cement concrete, by weight percentage, wherein:
[0019] Early strength component 40%,
[0020] Quick-setting component 22%,
[0021] 38% reduced water components,
[0022] Among them, the early-strength component is composed of calcium formate and calcium nitrate, and the weight ratio is 67.7%:32.3%. The quick-setting component is selected from aluminum sulfate; the water-reducing component is selected from polycarboxylate high-performance water reducer.
[0023] The preparation method of this embodiment is to weigh the admixture according to the weight percentage, use the internal mixing method, add it into water and stir it quickly to make the super early strength agent dissolve quickly.
[0024] The amount of super early strength agent is 2% of the cementitious material, the water-cement ratio of the concrete is 0.3, and the sand rate is 0.35. After the concrete is formed, the slump of the concrete a...
Embodiment 2
[0025] Embodiment two: a kind of super early strength agent of portland cement concrete, by weight percentage, wherein:
[0026] Early strength component 44%,
[0027] Quick-setting component 20%,
[0028] 36% reduced water component,
[0029] Among them, the early strength component is composed of calcium formate and calcium nitrite, and the weight ratio is 64.3%:35.7%; the quick-setting component is selected from aluminum sulfate; the water-reducing component is selected from polycarboxylate high-performance water reducer .
[0030] The preparation method of this embodiment is to weigh the admixture according to the weight percentage, use the internal mixing method, add it into water and stir it quickly to make the super early strength agent dissolve quickly.
[0031] The amount of super early strength agent is 2% of the cementitious material, the water-cement ratio of the concrete is 0.3, and the sand rate is 0.35. After the concrete is formed, the slump of the concrete ...
Embodiment 3
[0032] Embodiment three: a kind of super early strength agent of portland cement concrete, by weight percentage, wherein:
[0033] Early strength component 46%,
[0034] Quick-setting component 22%,
[0035] 32% water reduction component,
[0036] Among them, the early-strength component is composed of triethanolamine, calcium formate and calcium nitrate, and the weight ratio is 1%:66%:33%; the quick-setting component is aluminum sulfate; the water-reducing component is polycarboxylate High performance water reducer.
[0037] The preparation method of this embodiment is to weigh the admixture according to the weight percentage, use the internal mixing method, add it into water and stir it quickly to make the super early strength agent dissolve quickly.
[0038] The dosage of super early strength agent is 2.2% of the cementitious material, the water-cement ratio of the prepared concrete is 0.3, and the sand rate is 0.35. After the concrete is formed, the concrete slump and i...
PUM
Property | Measurement | Unit |
---|---|---|
compressive strength | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com