A kind of foamable rubber particles
A technology of rubber particles and foaming agents, applied in the field of high molecular polymers, can solve the problems of high energy consumption, high production cost, and poor fluidity of rubber materials, and achieve the effect of controllable physical properties, low production cost and soft texture
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] Ethylene-vinyl acetate copolymer 20 parts
[0019] POE elastomer 1 part
[0020] Foaming agent 1 part
[0021] Vulcanizing agent 1 part
[0022] Strengthening agent 10 parts
[0023] Dispersant 0.5 parts
[0024] Modified flow agent 1.5 parts
[0025] This formula is to meet the requirements of products with high wear resistance, high tensile resistance and microcellular foaming. The production steps are: first put the rubber composition, modified flow agent, reinforcing agent, and dispersant into the internal mixer for internal mixing, mix for 12 minutes, add foaming agent and vulcanizing agent, and mix for 5 minutes. The temperature of the internal mixer is 95°C, and then the rubber particles are formed after kneading and extrusion. Put the foamable rubber particles into the station-type injection molding machine, heat and pressurize the rubber particles to make it into a turbulent rubber material. The temperature of this process is 120°C and the pressure is 110...
Embodiment 2
[0029] Ethylene-vinyl acetate copolymer 15 parts
[0030] POE elastomer 10 parts
[0031] EPDM glue 10 parts
[0032] Filler 10 parts
[0033] Foaming agent 2 parts
[0034] Vulcanizing agent 1 part
[0035] Strengthening agent 10 parts
[0036] Dispersant 0.5 parts
[0037] Modified flow agent 1.5 parts
[0038] This formula is to meet the requirements of products with high elasticity, anti-aging, acid and alkali resistance, and light foaming, such as building and mechanical sealing products. The production steps are as follows: first put the rubber composition, modified flow agent, reinforcing agent, and dispersant into the internal mixer for internal mixing, mix for 8 minutes, add foaming agent and vulcanizing agent, and mix for 3 minutes. The temperature of the internal mixer is 90°C, and then the rubber particles are formed after kneading and extrusion. Put the foamable rubber particles into the station-type injection molding machine, heat and pressurize the rubbe...
Embodiment 3
[0042] POE elastomer 15 parts
[0043] EPDM glue 15 parts
[0044] Filler 15 parts
[0045] Foaming agent 5 parts
[0046] Vulcanizing agent 0.5 part
[0047] Strengthening agent 7.5 parts
[0048] Dispersant 0.5 parts
[0049] Modified flow agent 1.5 parts
[0050] This formula is to meet the requirements of products with high elasticity, high wear resistance and heavy foaming, such as shoe soles and slippers. The production steps are as follows: first put the rubber composition, modified flow agent, reinforcing agent, and dispersant into the internal mixer for internal mixing, mix for 10 minutes, add foaming agent and vulcanizing agent, and mix for 5 minutes. The temperature of the internal mixer is 95°C, and then the rubber particles are formed after kneading and extrusion. Put the foamable rubber particles into the station-type injection molding machine, heat and pressurize the rubber particles to make it into a turbulent rubber material. The temperature of this pro...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com