Diacetylene-class thermochromic ink and method for preparing same
A thermochromic ink and thermochromic technology, used in inks, household appliances, applications, etc., can solve the problems of ink containing toxic and harmful substances, secondary pollution, etc., and achieve uniform dispersion of color components, saving consumption, and simple equipment. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] A diacetylene thermosensitive color-changing ink is composed of the following raw materials in parts by mass:
[0030] 10 parts of 10,12-pentacosadiynoic acid;
[0031] 45 parts of tung oil;
[0032] Calcium carbonate 25 parts;
[0033] 15 parts of barium sulfate;
[0034] Annatto pigment 5 parts.
[0035] A preparation method of diacetylenic temperature-sensitive color-changing ink, comprising the following steps:
[0036] (1) Mixing: Add diacetylene-based thermochromic materials to tung oil, use an ink knife to manually stir, add annatto pigment while stirring as needed, and stir for 2 minutes to form a mixture;
[0037] (2) Heating: heat the mixture in a microwave oven for 15 seconds to raise the temperature of the mixture to 55°C, continue stirring manually with an ink knife for 1 minute, and heat it in the microwave oven again for 15 seconds to raise the temperature of the mixture to 55°C;
[0038] (3) Add filler: add calcium carbonate and barium sulfate to th...
Embodiment 2
[0041] A diacetylene thermosensitive color-changing ink is composed of the following raw materials in parts by mass:
[0042] 15 parts of 10,12-trisosadiynoic acid;
[0043] 50 parts of linseed oil;
[0044] 22 parts of calcium carbonate;
[0045] Barium sulfate 13 parts.
[0046] A preparation method of diacetylenic temperature-sensitive color-changing ink, comprising the following steps:
[0047] (1) Mixing: add diacetylenic thermochromic material to linseed oil, use ink knife to manually stir, and stir for 2 minutes to form a mixture;
[0048] (2) Heating: Heat the mixture in a microwave oven for 15s to raise the temperature of the mixture to 50°C, use an ink knife to continue stirring by hand for 2 minutes, put it into the microwave oven again and heat for 15s to raise the temperature of the mixture to 50°C;
[0049] (3) Add filler: add calcium carbonate and barium sulfate to the heated mixture at the same time, stir with an ink knife for 2-4 minutes, until the viscosi...
Embodiment 3
[0052] A diacetylene thermosensitive color-changing ink is composed of the following raw materials in parts by mass:
[0053] 5 parts of 10,12-pentacosadiynoic acid;
[0054] 5 parts of 10,12-trisosadiynoic acid;
[0055] 40 parts of tung oil;
[0056] Calcium carbonate 25 parts;
[0057] 10 parts of barium sulfate;
[0058] Capsanthin 5 parts.
[0059] A preparation method of diacetylenic temperature-sensitive color-changing ink, comprising the following steps:
[0060] (1) Mixing: Add diacetylene-based thermochromic materials to tung oil, use an ink knife to manually stir, add capsanthin while stirring as needed, and stir for 2 minutes to form a mixture;
[0061](2) Heating: heat the mixture in a microwave oven for 15 seconds to raise the temperature of the mixture to 60°C, continue to stir manually for 1 minute with an ink knife, and heat it in the microwave oven again for 15 seconds to raise the temperature of the mixture to 60°C;
[0062] (3) Add filler: add calcium...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com