Preparation method of thulium and europium single/co-doped lutetium gallium garnet phosphor
A gallium garnet and phosphor technology, applied in the field of luminescent materials, can solve the problems of difficulty in control, agglomeration of precursor powders, and difficulty in forming precursor powders with a sedimentation rate, and achieves a narrow emission peak, a simple production process, and easy ball milling. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] Embodiment 1 A kind of europium monodoped lutetium gallium garnet (LGG) fluorescent powder, chemical formula is Lu 2.98 Ga 5 o 12 :0.02Eu 3+ ;
[0025] 1) dissolving gallium oxide powder with concentrated nitric acid with a mass fraction of 69%; dissolving europium nitrate and lutetium nitrate in deionized water, mixing the two solutions to form a metal ion solution; wherein, Lu 3+ :Eu 3+ : Ga3+ The molar ratio is 2.98:0.02:5;
[0026] 2) Add citric acid to the metal ion mixed solution prepared in step 1, and mix well to obtain a mixed solution, wherein the molar ratio of citric acid to the sum of the contents of all metal ions is 1.5:1;
[0027] 3) Put the mixed solution in step 2 in a water bath at 80°C for 0.5h, until all of it turns into a pale yellow gel;
[0028] 4) Move the light yellow gel in step 3 into an oven, and keep the temperature at 250° C. for 2 hours to obtain dark brown bulky powder;
[0029] 5) The dark brown bulky powder obtained in step 4) i...
Embodiment 2
[0031] Embodiment 2 A kind of europium monodoped lutetium gallium garnet (LGG) fluorescent powder, its chemical formula is Lu 2.96 Ga 5 o 12 :0.04Eu 3+ .
[0032] 1) dissolving gallium oxide powder with concentrated nitric acid with a mass fraction of 69%; dissolving europium nitrate and lutetium nitrate in deionized water, mixing the two solutions to form a metal ion solution; wherein, Lu 3+ :Eu 3+ : Ga 3+ The molar ratio is 2.96:0.04:5;
[0033] 2) Add citric acid to the metal ion mixed solution prepared in step 1, and mix well to obtain a mixed solution, wherein the molar ratio of citric acid to the sum of the contents of all metal ions is 1.5:1;
[0034] 3) Put the mixed solution in step 2 in a water bath at 80°C for 1 hour until all of it turns into a pale yellow gel;
[0035] 4) Move the light yellow gel in step 3 into an oven, and keep the temperature at 250° C. for 4 hours to obtain dark brown bulky powder;
[0036] 5) The dark brown bulky powder obtained in st...
Embodiment 3
[0037] Embodiment 3 A kind of europium monodoped lutetium gallium garnet (LGG) fluorescent powder, its chemical formula is Lu 2.99 Ga 5 o 12 :0.01Eu 3+ .
[0038] 1) dissolving gallium oxide powder with concentrated nitric acid with a mass fraction of 69%; dissolving europium nitrate and lutetium nitrate in deionized water, mixing the two solutions to form a metal ion solution; wherein, Lu 3+ :Eu 3+ : Ga 3+ The molar ratio is 2.99:0.01:5;
[0039] 2) Add citric acid to the metal ion mixed solution prepared in step 1, and mix well to obtain a mixed solution, wherein the molar ratio of citric acid to the sum of the contents of all metal ions is 1.5:1;
[0040] 3) Put the mixed solution in step 2 in a water bath at 80°C for 0.8h, until all of it turns into a pale yellow gel;
[0041] 4) Move the light yellow gel in step 3 into an oven, and keep the temperature at 250° C. for 2 hours to obtain dark brown bulky powder;
[0042] 5) The black-brown bulky powder obtained in st...
PUM

Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com