A production process and blended yarn technology, which is applied in yarn, textile, papermaking, biochemical fiber treatment, etc., can solve the problems of low strength, poor wear resistance, rough hand feeling, etc., and achieve simplified production steps, optimized production process, and better hand feel. good effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] (a) Proportioning raw materials: prepare raw materials, including 25% wool, 25% rabbit hair, 35% cotton, and 15% chemical fiber;
[0020] (b) Opening process: use FA106 type opening machine to mix the raw materials, in which the speed of the needle roller is 510r / min, the speed of the beater is 750r / min, and the distance between the beater and the roller is 10mm;
[0021] (c) Carding process: FX256 combing machine is used to comb the raw materials, the speed is 190m / min, 170 tongs / min;
[0022] (d) Drawing process: draw frame FA322 is used to draw the yarn, and the speed is 250m / min;
[0023] (e) Coarse sanding process: roving the blended yarn with the roving frame RF4a;
[0024] (f) Spinning process: use spinning frame B583 to subdivide the blended yarn;
[0025] (g) Enzyme treatment step: 1398 protease is used to remove the gum on the blended yarn, the concentration is 6% owf, the bath ratio is 1:20, the pH value is 6.5, and the treatment temperature is 45°C. Processing time is...
Embodiment 2
[0031] (a) Proportioning raw materials: prepare raw materials, including 25% wool, 25% rabbit hair, 35% cotton, and 15% chemical fiber;
[0032] (b) Opening process: use FA106 type opening machine to mix the raw materials, in which the speed of the needle roller is 550r / min, the speed of the beater is 800r / min, and the distance between the beater and the roller is 10mm;
[0033] (c) Carding process: use FX256 combing machine to comb the raw materials, the speed is 250m / min, 250 tongs / min;
[0034] (d) Drawing process: draw frame FA322 is used to draw the yarn, and the speed is 400m / min;
[0035] (e) Coarse sanding process: roving the blended yarn with the roving frame RF4a;
[0036] (f) Spinning process: use spinning frame B583 to subdivide the blended yarn;
[0037] (g) Enzyme treatment process: using 1398 protease to remove the gum on the blended yarn, the concentration is 10% owf, the bath ratio is 1:30, the pH value is 7.5, and the treatment temperature is 55°C. Processing time is 3...
Embodiment 3
[0043] (a) Proportioning raw materials: prepare raw materials, including 25% wool, 25% rabbit hair, 35% cotton, and 15% chemical fiber;
[0044] (b) Opening process: The FA106 type opening machine is used to mix the raw materials. The speed of the needle roller is 530r / min, the speed of the beater is 780r / min, and the distance between the beater and the roller is 10mm;
[0045] (c) Carding process: use FX256 combing machine to comb the raw materials, the speed is 220m / min, 190 tongs / min;
[0046] (d) Drawing process: draw frame FA322 is used to draw the yarn, and the speed is 320m / min;
[0047] (e) Coarse sanding process: roving the blended yarn with the roving frame RF4a;
[0048] (f) Spinning process: use spinning frame B583 to subdivide the blended yarn;
[0049] (g) Enzyme treatment process: using 1398 protease to remove the gum on the blended yarn, the concentration is 8% owf, the bath ratio is 1:25, the pH value is 7, and the treatment temperature is 48°C. Processing time is 2.5h;...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology