Monascorubrin mordant dyeing method of silk textile
A technology of monascus rubin and dyeing method, which is applied in the field of light chemical industry, can solve the problems of poor dyeing quality and environmental protection, achieve the effects of improving dyeing percentage and color fastness, expanding application fields, and increasing dyeing affinity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Example 1. Monascus rubin rare earth mordant dyeing of silk fabrics under different mordant dyeing methods.
[0025] The dyeing process conditions are: start dyeing at 30°C, heat up at 2°C / min to 80°C, and keep warm for 60 minutes; after the dyeing process is completed, wash with water and dry.
[0026] As can be seen from Table 1: the present invention uses rare earth as a mordant, and the monascus red pigment mordant dyeing of silk fabrics, under the above three mordant methods, the best dyeing effect with the same bath mordant method, and the color is darker, indicating that Under the same-bath mordant dyeing method, monascus rubin and mordant can fully undergo complexation reaction. The second is pre-mordant dyeing, and the color of post-mordant dyeing is lighter, which is due to the inability of some mordants to fully complex with monascus rubin. At the same time, the experimental results show that when praseodymium chloride is used for monascus rubin dyeing, the ...
Embodiment 2
[0029] Embodiment 2, the influence of different mordant dosages on dyeing effect.
[0030] The dyeing process conditions are: start dyeing at 30°C, heat up at 2°C / min to 80°C, and keep warm for 60 minutes; after the dyeing process is completed, wash with water and dry.
[0031] Under the condition that the amount of monascus rubin is 2%owf, pH=3~4, bath ratio is 1:30, and the amount of praseodymium chloride is 0.5, 1, 1.5, 2g / L respectively, the same bath mordant dyeing method is adopted, according to the The above dyeing process conditions are used for dyeing, and then the dyeing percentage and K / S value are measured, and the statistical results are shown in Table 2.
[0032] Table 2. Effects of different mordant dosages on dyeing percentage and K / S value.
[0033] Mordant dosage / g·L -1
Dyeing percentage / %
K / S
0
56.84
2.5782
0.5
80.26
3.2366
1
87.61
4.8504
1.5
87.57
4.8361
2
87.68
4.9013
...
Embodiment 3
[0036] Embodiment 3, the influence of different dye liquor pH values on the dyeing effect.
[0037] The dyeing process conditions are: start dyeing at 30°C, heat up at 2°C / min to 80°C, and keep warm for 60 minutes; after the dyeing process is completed, wash with water and dry.
[0038] Under the conditions of monascus rubin dosage 2%owf, praseodymium chloride concentration 1g / L, bath ratio 1:30, and pH 3; The dyeing process conditions were dyed, and the dyeing percentage and K / S value were measured. The statistical results are shown in Table 3.
[0039] Table 3. Effects of different pH values on dyeing percentage and K / S value.
[0040] pH
Dyeing percentage / %
K / S
3
87.61
4.8504
5
81.32
3.6514
7
79.28
3.2824
9
57.81
2.7146
11
32.46
1.8044
[0041] .
[0042] It can be seen from Table 3 that the dyeing percentage and k / S value decrease with the increase of pH value, which shows that under...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com