Repair-proof welded connection technology of inner walls of plastic-coated steel tubes
A technology for welded connection and plastic-coated steel pipes, which is applied to non-detachable pipe connections, pipes/pipe joints/fittings, passing components, etc., which can solve the problems of reduced fluid cross-section on the inner wall of steel pipes, difficulties in the promotion and application of plastic-coated steel pipes, and increased costs. , to achieve the effect of reducing concealed operations and good technical and economic benefits
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] Repair-free welding connection process for the inner wall of plastic-coated steel pipes, such as Figure 1 to Figure 4 As shown, the welding connection process is as follows:
[0033] a. Derusting steel pipes 1 and 2;
[0034] b. Steel pipe 1, 2 port thermal spraying metal coating;
[0035] c. Make a thin-walled stainless steel sleeve 3;
[0036] d. Put the thin-walled stainless steel sleeve 3 into the steel pipes 1 and 2 and make the thin-wall stainless steel sleeve 3 tightly line the inner walls of the steel pipes 1 and 2 by expanding the tube;
[0037] e. The end of the thin-walled stainless steel sleeve 3 is turned over according to the shape of the cutout of the steel pipe 1 to form a flanging 31;
[0038] f. The inner and outer walls of steel pipes 1 and 2 are coated with step coatings 6 and 7;
[0039] g. Transport the steel pipes 1 and 2 covered with thin-walled stainless steel sleeves 3 to the site;
[0040] h. The thin-walled stainless steel sleeves 3 are...
Embodiment 2
[0052] Repair-free welding connection process for the inner wall of plastic-coated steel pipes, such as Figure 1 to Figure 4 As shown, the welding connection process is as follows:
[0053] a. Derusting steel pipes 1 and 2;
[0054] b. Steel pipe 1, 2 port thermal spraying metal coating;
[0055] c. Make a thin-walled stainless steel sleeve 3;
[0056] d. Put the thin-walled stainless steel sleeve 3 into the steel pipes 1 and 2 and make the thin-wall stainless steel sleeve 3 tightly line the inner walls of the steel pipes 1 and 2 by expanding the tube;
[0057] e. The end of the thin-walled stainless steel sleeve 3 is turned over according to the shape of the cutout of the steel pipe 1 to form a flanging 31;
[0058] f. The inner and outer walls of steel pipes 1 and 2 are coated with step coatings 6 and 7;
[0059] g. Transport the steel pipes 1 and 2 covered with thin-walled stainless steel sleeves 3 to the site;
[0060] h. The thin-walled stainless steel sleeves 3 are...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com