Method for preparing repairing material of antibacterial degradable active nanometer composite bionic tone tissue
A nano-composite and tissue repair technology, applied in the field of biomedical engineering, can solve the problems of multi-animal experiments and clinical trials, and achieve the effects of good environment, high output, and simple operation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] The preparation method of the antibacterial and degradable active nanocomposite biomimetic bone tissue repair material is characterized in that it includes the following steps:
[0034] A. Dissolve 8g of conventional hydroxyapatite (HA) in 20ml of 5M hydrochloric acid solution, and mix with 10ml of 2% minocycline in 0.1M hydrochloric acid solution into 100ml of 2% gelatin aqueous solution.
[0035] B. Keep the above mixed solution obtained in a silicone oil reaction bath at 40°C under continuous stirring conditions. Adjust the pH value of the reaction system to 7-8 with 1M NaOH, and react for 2 hours.
[0036] C. After the reaction is complete, adjust the pH value of the reaction system to 7 dropwise with 0.1M hydrochloric acid and sodium hydroxide and keep it stable. Then stand at room temperature and age for 24 hours.
[0037] D. The final reaction product is centrifuged, and the supernatant is discarded; the precipitate is washed with deionized water, centrifuged, ...
Embodiment 2
[0044]A, 9.9721g of calcium chloride (CaCl 2 ) and 5.7309g of sodium dihydrogen phosphate (NaH 2 PO 4 ) was dissolved in 20ml of 1M hydrochloric acid solution. Dissolve 0.2 g of minocycline in 10 ml of 0.1 M hydrochloric acid solution; then mix the prepared calcium / phosphorus solution and minocycline solution into 100 ml of 2% gelatin aqueous solution respectively.
[0045] B. Keep the above mixed solution obtained in a silicone oil reaction bath at 40°C under continuous stirring conditions. Adjust the pH value of the reaction system to 7-8 with 1M NaOH, and react for 2 hours.
[0046] C. After the reaction is complete, adjust the pH value of the reaction system to 7 dropwise with 0.1M hydrochloric acid and sodium hydroxide and keep it stable. Then stand at room temperature and age for 24 hours.
[0047] D. The final reaction product is centrifuged, and the supernatant is discarded; the precipitate is washed with deionized water, centrifuged, and the operation is repeated...
Embodiment 3
[0049] A, 4.51481g of calcium hydroxide (Ca(OH) 2 ) and 5.7309g of sodium dihydrogen phosphate (NaH 2 PO 4 ) was dissolved in 20ml of 1M hydrochloric acid solution. Dissolve 0.2 g of minocycline in 10 ml of 0.1 M hydrochloric acid solution; then mix the prepared calcium / phosphorus solution and minocycline solution into 100 ml of 2% gelatin aqueous solution respectively.
[0050] B. Keep the above mixed solution obtained in a silicone oil reaction bath at 40°C under continuous stirring conditions. Adjust the pH value of the reaction system to 7-8 with 1M NaOH, and react for 2 hours.
[0051] C. After the reaction is complete, adjust the pH value of the reaction system to 7 dropwise with 0.1M hydrochloric acid and sodium hydroxide and keep it stable. Then stand at room temperature and age for 24 hours.
[0052] D. The final reaction product is centrifuged, and the supernatant is discarded; the precipitate is washed with deionized water, centrifuged, and the operation is rep...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com