example 1
[0020] Castor oil 90kg
[0021] T603 75kg
[0022] White carbon black and heavy calcium carbonate mixture 290kg
[0023] Thickener 25kg
[0024] Antifungal agent 6.0kg
[0025] Dispersant 4.0kg
[0026] Bamboo fiber 10kg
[0027] The preparation process is as follows: First, mix 90kg of castor oil, 75kg of T603, 25kg of thickener, 6.0kg of antifungal agent, and 4.0kg of wetting and dispersing agent in a mixer at room temperature, and then add 290kg of The mixture of white carbon black and heavy calcium carbonate is mixed evenly, and finally 10kg of bamboo fiber is added, and fully stirred and kneaded for not less than 90 minutes.
example 2
[0029] Castor oil 125kg
[0030] T603 78.5kg
[0031] Bentonite and superfine calcium carbonate mixture 250kg
[0032] Thickener 25kg
[0033] Antifungal agent 4.0kg
[0034] Dispersant 2.5kg
[0035] Bamboo fiber 15kg
[0036] The preparation process is as follows: First, mix 125kg of castor oil, 78.5kg of T603, 25kg of thickener, 4.0kg of antifungal agent, and 2.5kg of wetting and dispersing agent in a mixer at room temperature, and then add them in batches 250kg of bentonite and superfine calcium carbonate mixture are mixed evenly, and finally 15kg of bamboo fiber is added, and fully stirred and kneaded for no less than 90 minutes.
example 3
[0038] soybean oil 75kg
[0039] T613 85kg
[0040] White carbon black and mica powder mixture 250kg
[0041] Thickener 50kg
[0042] Antifungal agent 5.0kg
[0043] Dispersant 5.0kg
[0044] Bamboo fiber 30kg
[0045] The preparation process is as follows: First, mix 75kg of soybean oil, 85kg of T613, 50kg of thickener, 5.0kg of antifungal agent, and 5.0kg of wetting and dispersing agent in a mixer at room temperature, and then add 250kg of Mix the white carbon black and mica powder mixture evenly, and finally add 30kg of bamboo fiber, and fully stir and knead for no less than 90 minutes.
PUM
Property | Measurement | Unit |
---|---|---|
Evaporation rate | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com