Waterborne PU color-change resin for synthetic leather
A synthetic leather and resin technology, applied in fiber processing, textiles and papermaking, etc., can solve the comprehensive effects of synthetic leather discoloration, viscosity, stability, touch feeling, etc. and other problems, to achieve the effect of excellent comprehensive effect, firm bonding and full hand feeling.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] 1. The water-based PU color-changing resin for synthetic leather is composed of the following raw materials: 100 kg of aliphatic polyurethane emulsion (30% solid content), 80 kg of ordinary tap water, 20 kg of silica color-changing powder, 7 kg of matting powder, and amino silicone oil slip agent 20 kg, emulsifying wax 20 kg, water-based polyurethane thickener 3 kg, silicone defoamer 20 kg, silicone leveling agent 3 kg.
[0027] 2. The preparation method of the water-based PU discoloration resin for synthetic leather of the present invention is as follows:
[0028] ① Select 100 kg of aliphatic polyurethane emulsion (30% solid content) according to the above ratio, 80 kg of ordinary tap water, 20 kg of silica discoloration powder, 7 kg of matting powder, 20 kg of amino silicone oil slip agent, 20 kg of emulsifying wax, organic 20 kg of silicon defoamer, 3 kg of silicone leveling agent, stirred for 2 hours, fully mixed, and set aside;
[0029] ② Grinding and filtering th...
Embodiment 2
[0035] 1. The water-based PU color-changing resin for synthetic leather is composed of the following raw materials: 90 kg of aromatic polyurethane emulsion (30% solid content), 80 kg of ordinary tap water, 18 kg of silica color-changing powder, 10 kg of matting powder, and amino silicone oil slip agent 15 kg, emulsifying wax 15 kg, non-ionic polyurethane polymer 4 kg, silicone defoamer 10 kg, silicone leveling agent 2 kg.
[0036] 2. The preparation method of the water-based PU discoloration resin for synthetic leather of the present invention is as follows:
[0037] ① Select 90 kg of aromatic polyurethane emulsion (30% solid content) according to the above ratio, 80 kg of ordinary tap water, 18 kg of silica discoloration powder, 10 kg of matting powder, 15 kg of amino silicone oil slip agent, 15 kg of emulsifying wax, organic 10 kg of silicon defoamer, 2 kg of silicone leveling agent, stirred for 2 hours, fully mixed, and set aside;
[0038] ② Grinding and filtering the reac...
Embodiment 3
[0044] 1. The water-based PU color-changing resin for synthetic leather is composed of the following raw materials: 70 kg of aliphatic polyurethane dispersion (30% solid content), 60 kg of ordinary tap water, 12 kg of silica color-changing powder, 4 kg of matting powder, and smooth amino silicone oil 10 kg of agent, 10 kg of emulsifying wax, 2 kg of non-ionic polyurethane polymer, 4 kg of silicone defoamer, and 1 kg of silicone leveling agent.
[0045] 2. The preparation method of the water-based PU discoloration resin for synthetic leather of the present invention is as follows:
[0046] ①Select 70 kilograms of aliphatic polyurethane dispersion (30% solid content) according to the above ratio, 60 kilograms of ordinary tap water, 12 kilograms of silicon dioxide discoloration powder, 4 kilograms of matting powder, 10 kilograms of amino silicone oil slippery agent, 10 kilograms of emulsifying wax, 4 kg of silicone defoamer, 1 kg of silicone leveling agent, stirred for 2 hours, f...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com