A technology of powder coating and heat insulating powder, applied in powder coating, cement coating, coating, etc., which can solve the problem of heat insulation effect discount, heat insulation performance, and aging resistance that are not as good as foreign similar products, and the thickness of ordinary heat insulation coatings Limitation and other issues, to achieve the effect of easy to use, excellent heat insulation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] A kind of water-based heat-insulating powder coating, its water-based heat-insulating powder component mass (kg) is as follows:
[0017] Nanoscale composite titanate thermal insulation powder 20kg
[0018] Composite silica-aluminate 30kg
[0019] Polypropylene monomer-polyvinyl alcohol 30kg
[0020] Titanium dioxide 18kg
[0021] Light calcium carbonate 2kg
[0022] The above components are fully stirred by a mixer to obtain a water-based heat-insulating powder.
[0023] Mix the above 100kg of water-based heat-insulating powder with 50kg of water to adjust to a suitable viscosity to obtain a water-based heat-insulating coating.
[0024] Brush the water-based heat-insulating paint on the 20×20×1cm cement board with a film thickness of 100цm. After one hour of infrared light irradiation, the temperature difference between the top and the back of the cement board reaches 25°C.
Embodiment 2
[0026] A water-based heat-insulating powder coating, the water-based heat-insulating powder component mass percent is:
[0027] Nanoscale composite titanate thermal insulation powder 5kg
[0028] Composite silica-aluminate 65kg
[0029] Polypropylene monomer-polyvinyl alcohol 10kg
[0030] Titanium dioxide 15kg
[0031] Light calcium carbonate 5kg
[0032] The above components are fully stirred by a mixer to obtain a water-based heat-insulating powder.
[0033] Mix the above 100kg of water-based heat-insulating powder with 80kg of water to adjust to an appropriate viscosity to obtain a water-based heat-insulating coating.
[0034] Brush the water-based thermal insulation paint on the polypropylene plastic board to test its thermal insulation effect at 25°C.
Embodiment 3
[0036] A water-based heat-insulating powder coating, the water-based heat-insulating powder component mass percent is:
[0037] Nanoscale composite titanate thermal insulation powder 14kg
[0038] Composite silica-aluminate 48kg
[0039] Polypropylene monomer-polyvinyl alcohol 20kg
[0040] Titanium dioxide 14kg
[0041] Light calcium carbonate 4kg
[0042] The above components are fully stirred by a mixer to obtain a water-based heat-insulating powder.
[0043] Mix the above 100kg of water-based heat-insulating powder with 65kg of water to adjust to an appropriate viscosity to obtain a water-based heat-insulating coating.
[0044] Paint the water-based heat-insulating paint on the inside of the cement pool, and there will be no water seepage for 720 hours.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com