Method for preparing tourmaline functional ceramic filter element
A technology of functional ceramics and tourmaline, applied in the field of preparation of tourmaline functional ceramic filter elements, can solve the problems of waste of resources and low utilization rate, and achieve the effect of increasing the contact area
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Its implementation formula is
[0021] Tourmaline powder 100 parts (1μm)
[0022] Additive sodium tripolyphosphate 10 parts
[0023] 15 parts of water
[0024] After mixing the tourmaline powder additive sodium tripolyphosphate and water according to the above formula, mechanically stir for 30 minutes to make a composite base material, press the prepared composite base material into a sheet in a mold, and make a tourmaline functional ceramic filter element green body; After demoulding, the green body is further dried and sintered at a temperature of 700°C and held for 1 hour. After cooling, a sheet-shaped porous tourmaline filter element is obtained. The filter element has a pore size of 0.2 μm, a porosity of 28%, a diameter of 123 mm, and a thickness of 6 mm.
[0025] The tourmaline ceramic filter element made by this embodiment is an ideal functional ceramic for water treatment. It can not only be used for water filtration, filter out harmful substances such as bact...
Embodiment 2
[0027] Its implementation formula is
[0028] Tourmaline powder 60 parts (6μm)
[0029] Excipients Medical stone 40 parts (10μm)
[0030] Additive sodium silicate 2 parts
[0031] 25 parts of water
[0032] According to the above formula, mix tourmaline powder, auxiliary material medical stone and additive sodium silicate with water, and mechanically stir for 1-4 hours to make a composite base material, and press the prepared composite base material into a tubular shape in a mold to make tourmaline Functional ceramic filter green body; after demoulding, the green body is further dried and sintered at a temperature of 1100°C, holding time for 1 hour, and the tubular porous tourmaline medical stone composite filter element is obtained after cooling.
[0033] Medical stone is named by ancient Chinese medical scientists based on its appearance resembling rice balls cooked from barley rice. It is the earliest natural mineral medicinal stone used in my country. It is a weathered...
Embodiment 3
[0036] Its implementation formula is
[0037] Tourmaline powder 60 parts
[0038] Excipients Zeolite 20 parts
[0039] Additive sodium phosphate 2 parts
[0040] 12 parts of water
[0041] According to the above formula, mix tourmaline powder, auxiliary material zeolite and additive sodium silicate with water, stir mechanically for 1-4 hours to make composite base material, and press the prepared composite base material into a tubular shape in a mold to make tourmaline functional ceramics The green body of the filter element; after demoulding, the green body is further dried and sintered at a temperature of 1200°C, with a holding time of 1 hour, and a tubular porous tourmaline filter element is obtained after cooling.
[0042] Zeolite is a family of hydrous aluminosilicate minerals with framework structure, which is composed of aluminosilicate framework, pores, holes and cations in the framework, and water molecules existing in solid phase. Si in a silicon-oxygen tetrahedr...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com