A production method and technology of colored bricks, applied in chemical instruments and methods, manufacturing tools, clay preparation devices, etc., can solve the problems of no water permeability, ventilation and heat dissipation, single color and single tone of a single colored brick, and achieve excellent flexural resistance Compressive strength, positive social benefits, and the effect of maintaining ecological balance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] The following takes the production of 10 square meters of 300*150*60cm yellow red and black magic color tiles as an example to describe in detail.
[0032] The prepared magic color surface color brick, each component and its weight percentage are:
[0033] First Layer Fabric: Diamond Rice 70.92%
[0034] Ordinary Portland PO425 cement 23.64% (gray cement or white cement)
[0035] Iron oxide pigment 0.71%
[0036] Water 4.73%
[0037] Second layer fabric: finely washed river sand 70.92%
[0038] Ordinary Portland PO425 cement 23.64% (gray cement or white cement)
[0039] Elements Iron Oxide Pigment 0.71%
[0040] Water 4.73%
[0041] Base material: fine washed river sand 47.62%
[0042] Selected Guami Stone 31.75%
[0043] Ordinary Portland PO425 cement 15.87%
[0044] Water 4.76%
[0045] Its production method is as follows:
[0046] (1) Prepare the first layer of fabric...
Embodiment 2
[0055] The prepared magic color surface color brick, each component and its weight percentage are:
[0056] First Layer Fabric: Diamond Rice 70%
[0057] Ordinary Portland PO425 cement 24% (gray cement or white cement)
[0058]Iron Oxide Pigment 1%
[0059] water 5%
[0060] Second Layer Fabric: 70% Washed River Sand
[0061] Ordinary Portland PO425 cement 24% (gray cement or white cement)
[0062] Elements Iron Oxide Pigment 1%
[0063] water 5%
[0064] Base material: finely washed river sand 47%
[0065] Selected Guami Stone 32%
[0066] Ordinary Portland cement PO425 16%
[0067] water 5%
[0068] Its preparation method is different from Example 1 in that the component content in each step is adjusted according to the above ratio, the male mold is pressed down and pre-vibrated for 3 seconds in the step (4), and the natural air-drying is 28 hours in the step (6).
Embodiment 3
[0070] The difference from Example 1 is that
[0071] The prepared magic color surface color brick, each component and its weight percentage are:
[0072] First Layer Fabric: Diamond Rice 71%
[0073] Ordinary Portland PO425 cement 23% (gray cement or white cement)
[0074] Iron Oxide Pigment 1%
[0075] water 5%
[0076] Second Layer Fabric: Washed River Sand 71%
[0077] Ordinary Portland PO425 cement 23% (gray cement or white cement)
[0078] Elements Iron Oxide Pigment 1%
[0079] water 5%
[0080] Base material: 50% fine washed river sand
[0081] Selected Guami Stone 31%
[0082] Ordinary Portland cement PO425 15%
[0083] water 4%
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com