A pine wood, neutral technology, applied in pressure impregnation and other directions, can solve the problems of difficulty, it is difficult to accurately reflect the permeability characteristics of the degreasing solution of large-size specimens, and the permeability of the degreasing solution varies greatly, achieving low production cost, physical mechanics. The effect of small property degradation and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] (1) Prepare degreasing liquid: mix ethanol and benzene according to the volume ratio of 1:1 to obtain a mixed solvent, then dilute the mixed solvent with water according to the volume ratio of 1:99 to prepare a degreasing liquid;
[0021] (2) Canning: According to the volume of pine wood / volume of degreasing liquid is 1:1, put the degreasing liquid and larch board into a high-pressure degreasing tank (required to withstand the pressure of 3MPa);
[0022] (3) Degreasing treatment: heat up to 110°C at the fastest speed, keep it warm for 8 hours, make the degreasing depth reach 5-6cm, and keep the color of fresh pine wood; then cool to 50°C, discharge the liquid, and recover the rosin; drain the liquid Finally, open the degreasing tank and unload the pine wood. After degreasing, the degreasing rate reaches more than 80%, the color presents the color of fresh material, and the change of physical and mechanical properties does not exceed 8%.
Embodiment 2
[0024] (1), prepare degreasing liquid: mix ethanol and benzene according to volume ratio 9: 1, obtain mixed solvent, then dilute mixed solvent with water according to volume ratio 1: 9, be mixed with degreasing liquid;
[0025] (2), canning: according to pine wood volume / skimming liquid volume is 1: 10, put degreasing liquid and masson pine plate into high-pressure degreasing tank (require to bear the pressure of 3MPa);
[0026] (3) Degreasing treatment: heat up to 160°C at the fastest speed, keep warm for 4 hours, make the degreasing depth reach 5-6cm, and keep the color of fresh pine wood; then cool to 80°C, discharge the liquid, and recover the rosin; After the liquid, open the skim tank and unload the pine. After degreasing, the degreasing rate reaches more than 80%, the color presents the color of fresh material, and the change of physical and mechanical properties does not exceed 8%.
Embodiment 3
[0028] (1), prepare degreasing liquid: mix ethanol and benzene according to volume ratio 3: 1, obtain mixed solvent, then dilute mixed solvent with water according to volume ratio 1: 66, be mixed with degreasing liquid;
[0029] (2), canning: according to the volume of pine wood / volume of degreasing liquid is 1:0.5, put the degreasing liquid and slash pine plate into high-pressure degreasing tank (required to withstand the pressure of 3MPa);
[0030] (3) Degreasing treatment: heat up to 140°C at the fastest speed, keep warm for 6 hours, make the degreasing depth reach 5-6cm, and keep the color of fresh pine wood; then cool to 60°C, discharge the liquid, and recover the rosin; After the liquid, open the skim tank and unload the pine. After degreasing, the degreasing rate reaches more than 80%, the color presents the color of fresh material, and the change of physical and mechanical properties does not exceed 8%.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com