Water resin craft article colour drawing paint and preparation process thereof
A water-based resin and handicraft technology, applied in the direction of art coatings, etc., to achieve the effects of good weather resistance, improved chemical resistance and mechanical resistance, and simple production process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Weigh 40 parts (weight percentage, the same below) water-based polyacrylate, 5 parts n-butanol, 5 parts water-based metal complex dye solution (Red-10, solid content 30%, provided by Guangdong Sanbao Chemical Co., Ltd.), 30 parts Deionized water, 20 parts of water-based crosslinking agent for use
[0022] Component 1: First put 40 parts of water-based polyacrylate into the stirring tank, start the mixer, and then slowly add 5 parts of n-butanol, after stirring, add 30 parts of deionized water and stir for about 5 minutes, then add 5 parts Red-10 metal complex dye solution, stir for about 5 minutes.
[0023] Component 2: Water-based crosslinking agent biuret polyisocyanate.
[0024] Before the paint is applied, take 80 parts of component one and 20 parts of component two, stir and mix thoroughly, leave it for a while, and then apply. Apply the paint to the clean resin crafts, put it at room temperature and ventilation for 5 minutes to dry on the surface, and dry in 2.5 hours...
Embodiment 2
[0028] Weigh 40 parts (weight percentage, the same below) water-based polyacrylate, 5 parts n-butanol, 5 parts water-based metal complex dye solution (Blue-03, solid content 30%, provided by Guangdong Sanbao Chemical Co., Ltd.), 30 parts Deionized water, 20 parts of water-based crosslinking agent for use
[0029] Component 1: First put 40 parts of water-based polyacrylate into the stirring tank, start the mixer, and then slowly add 5 parts of n-butanol, after stirring, add 30 parts of deionized water and stir for about 5 minutes, then add 5 parts Blue-03 metal complex dye solution, stir for about 5 minutes.
[0030] Component 2: Water-based crosslinking agent biuret polyisocyanate.
[0031] Before the paint is applied, take 80 parts of component one and 20 parts of component two, stir and mix thoroughly, leave it for a while, and then apply. Apply the paint to the clean resin crafts, put it at room temperature and ventilation for 5 minutes to dry on the surface, and dry in 2.5 hou...
Embodiment 3
[0035] Weigh 45 parts (weight percentage, the same below) water-based polyacrylate, 3 parts n-butanol, 5 parts water-based metal complex dye solution (Red-10, solid content 30%, provided by Guangdong Sanbao Chemical Co., Ltd.), 0.2 parts Byk020 defoamer (manufactured by BYK Chemie, Germany), 24.3 parts of ion-free water, and 22.5 parts of water-based crosslinking agent are ready for use.
[0036] Component 1: First put 45 parts of water-based polyacrylate into the stirring tank, start the mixer, and then slowly add 3 parts of n-butanol, after stirring, add 24.3 parts of deionized water and stir for about 5 minutes, then add 5 parts Red-10 metal complex dye solution, stir for about 5 minutes.
[0037] Component 2: Water-based crosslinking agent biuret polyisocyanate.
[0038] Before the coating is applied, take 77.5 parts of component one and 22.5 parts of component two, stir and mix thoroughly, leave it for a while, and then apply. Apply the paint to the clean resin crafts, place ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com