Autoclaved aerated concrete block made of gold tailings and its production process
A technology of concrete blocks and autoclaved gas filling, applied in the direction of climate sustainability, sustainable waste treatment, solid waste management, etc., can solve the problems of excessive radioactive substances, tight supply and demand of raw materials, and endangering human health, and achieve antifreeze Strong performance, no radioactive hazard, environmental protection and radioactive hazard effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Example 1: gold tailings autoclaved aerated concrete block, the main raw materials are gold tailings slag, cement, quicklime and water; according to the weight percentage, the main raw material formula ingredient ratio is: gold tailings slag 60%, cement 10% , 24.95% quicklime, 0.05% aluminum powder, 5% phosphogypsum powder, and the amount of water used is enough to make the gold tailings slag grinding fine slurry concentration meet the requirements;
[0022] Gold tailings slag: chemical composition silica content of 70-90%; cement: PC32.5R calcium oxide content of more than 70%; quicklime: calcium oxide content of more than 80%.
[0023] Silica and calcium oxide are subjected to hydrothermal reaction under autoclaved curing conditions to produce new silicate materials, which have a certain strength; aluminum powder acts as a gas generator; phosphogypsum powder is produced during the hydrothermal reaction process Acts as a retarder.
[0024] The production method flow i...
Embodiment 2
[0031] Embodiment 2: The difference between the gold tailings autoclaved aerated concrete block and the production method of the present embodiment and the embodiment 1: according to the percentage by weight, the ingredients ratio of the raw material formula is: gold tailings slag 70%, cement 6%, quicklime 21.97%, 0.03% aluminum powder, 2% phosphogypsum powder, and the amount of water used is enough to make the gold tailings slag grinding slurry concentration meet the requirements.
Embodiment 3
[0032] Embodiment 3: The difference between the gold tailings autoclaved aerated concrete block of this embodiment and its production method and that of Embodiment 1: according to the percentage by weight, the ingredients of the raw material formula are as follows: 66.99% of gold tailings slag, 9% of cement, quicklime 20%, aluminum powder 0.01%, phosphogypsum powder 4%, and the amount of water used is enough to make the gold tailings slag grinding slurry concentration meet the requirements.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com