A technology of active agent and nut, which is applied in the field of resistance welding, can solve the problems affecting the assembly quality of the whole workpiece and even the whole vehicle, short welding time of nut projection welding, and small nucleation size, etc., so as to improve welding consistency, short welding time, Effect of increasing weld nugget penetration
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0026] A kind of preparation method of welding auxiliary active agent, by mass percentage, its preparation steps are as follows:
[0027] 1) The powder and the binder are mixed according to the mass ratio of 1:4~6 to form the active agent;
[0028] 2) Dilute the active agent in step 1) with acetone at a ratio of 1.5 to 3:1;
[0029] The powder includes the following components by mass percentage: carbon black 50%-65%, CaF2 4%-10%, TiO2 16%-25%, Mn 15%-27%.
[0030] A method for increasing welding penetration nut projection welding, comprising the following steps:
[0031] 1) Preparation of auxiliary active agent;
[0032] 2) Place the prepared active agent in the active agent box;
[0033] 3) Install the active agent box on the nut conveyor conveying structure;
[0034] 4) When performing nut projection welding, the nut passes through the activator box during the conveying process, so that the nut bumps are dipped into the activator.
Embodiment 1
[0036] Weigh the powder according to the following mass percentages: carbon black 50%, CaF2 5%, TiO2 18%, Mn 22%. After mixing the powder evenly, mix it with the binder at a ratio of 1:4 to 6 to form an active agent, then dilute the active agent with acetone at a ratio of 1.5 to 3:1 for nut projection welding.
Embodiment 2
[0038] Weigh the powder according to the following mass percentages: carbon black 56%, CaF2 6%, TiO2 17%, Mn 21%. After mixing the powder evenly, mix it with the binder at a ratio of 1:4 to 6 to form an active agent, then dilute the active agent with acetone at a ratio of 1.5 to 3:1 for nut projection welding.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com