One-step method for preparing pyrochlore-phase borosilicate glass-ceramic solidified substrate
A silicate glass and ceramic solidification technology, applied in radioactive purification, nuclear engineering, etc., can solve the problems of difficult realization of high-level radioactive nuclear waste solidification treatment engineering, unfavorable control of crystal phase and composition, and unsuccinct process, etc., to achieve Excellent chemical stability, uniform crystal phase size, and good structural stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] A method for preparing a pyrochlore-phase borosilicate glass-ceramic solidified base material in one step, comprising the following steps:
[0028] a. Ingredients: Na 2 SiO 3 , CaF 2 、H 3 BO 3 , Nb 2 o 5 、TiO 2 、Nd 2 o 3 , Al(OH) 3 , SiO 2 as raw material, according to Na 2 SiO 3 33.8 parts by weight, CaF 2 8.8 parts by weight, H 3 BO 3 6.2 parts by weight, Nb 2 o 5 21.6 parts by weight, TiO 2 4.5 parts by weight, Nd 2 o 3 15.0 parts by weight, Al(OH) 3 4.3 parts by weight, SiO 2 The proportioning of 5.8 parts by weight gets each raw material;
[0029]b. Mixing: put each raw material into a ball milling equipment with absolute ethanol as a medium for ball milling and mixing for 4 hours to obtain a homogeneously mixed compound slurry;
[0030] c. Drying: Dry the compound slurry in a constant temperature drying oven for 24 hours, discharge the absolute ethanol and water in the raw materials, and prepare the compound;
[0031] d. Melting: Heat...
Embodiment 2
[0034] A method for preparing a pyrochlore-phase borosilicate glass-ceramic solidified base material in one step, comprising the following steps:
[0035] a. Ingredients: Na 2 SiO 3 , CaF 2 、H 3 BO 3 , Nb 2 o 5 、TiO 2 、Nd 2 o 3 , Al(OH) 3 , SiO 2 as raw material, according to Na 2 SiO 3 34.6 parts by weight, CaF 2 7.7 parts by weight, H 3 BO 3 7.0 parts by weight, Nb 2 o 5 22.4 parts by weight, TiO 2 4.4 parts by weight, Nd 2 o 3 14.5 parts by weight, Al(OH) 3 3.4 parts by weight, SiO 2 The proportioning of 6.0 parts by weight gets each raw material;
[0036] b. Mixing: put each raw material into a ball milling equipment with absolute ethanol as a medium for ball milling and mixing for 6 hours to obtain a homogeneously mixed compound slurry;
[0037] c. Drying: Dry the batch slurry in a constant temperature drying oven for 36 hours, and discharge the absolute ethanol and water in the raw materials to prepare the batch.
[0038] d. Melting: Heat th...
Embodiment 3
[0041] A method for preparing a pyrochlore-phase borosilicate glass-ceramic solidified base material in one step, comprising the following steps:
[0042] a. Ingredients: Na 2 SiO 3 , CaF 2 、H 3 BO 3 , Nb 2 o 5 、TiO 2 、Nd 2 o 3 , Al(OH) 3 , SiO 2 as raw material, according to Na 2 SiO 3 34.9 parts by weight, CaF 2 8.4 parts by weight, H 3 BO 3 6.9 parts by weight, Nb 2 o 5 24.6 parts by weight, TiO 2 3.5 parts by weight, Nd 2 o 3 12.8 parts by weight, Al(OH) 3 3.4 parts by weight, SiO 2 The proportioning of 5.5 parts by weight gets each raw material;
[0043] Others are the same as embodiment 1 or 2, omitted.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com