Purification method of high-purity quartz sand with SiO2 purity more than or equal to 99.99%
A technology of high-purity quartz sand and a purification method, which is applied in the field of purification of high-purity quartz sand with SiO2 purity ≥ 99.99%, can solve the problems of low added value of quartz sand and the inability to maximize economic benefits, etc., so as to improve product purity and improve The effect of economic benefits
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] Use 60-200 mesh quartz sand powder produced by a quartz sand company in Heyuan City, Guangdong Province as raw material
[0037] 1 Flotation: first flotation to remove feldspar impurities, and then flotation to remove layered aluminosilicate mineral impurities
[0038] Using hydrofluoric acid and NaOH as the pH regulator, dodecylamine as the trapping agent, and No. 2 oil as the foaming agent, the quartz sand powder is subjected to three flotations under the condition of pH 2.0 to 3.0 to remove feldspar mineral impurities; and then Hydrochloric acid and sodium hydroxide are used as pH regulators, quaternary ammonium salt cations (tetradecyltrimethylammonium chloride) are used as capture agents, and phenethyl ester oil is used as foaming agents, under the condition of pH 2.0-3.0 Three times of flotation to remove layered aluminosilicate mineral impurities such as kaolin, illite, pyrophyllite, etc., then washed with water until neutral, dehydrated, and dried for later use....
Embodiment 2
[0052] Take the 60-200 mesh quartz sand powder produced by a quartz sand company in Lankou, Heyuan City, Guangdong Province as an example
[0053] 1 Flotation: Remove feldspar impurities by conventional flotation methods;
[0054] Using hydrofluoric acid and KaOH as the pH regulator, dodecylamine as the capture agent, and No. 2 oil as the foaming agent, the quartz sand powder is subjected to 4 times of flotation under the condition of pH 2.0 to 3.0 to remove feldspar mineral impurities; Then hydrochloric acid and sodium hydroxide are used as pH regulators, quaternary ammonium salt cation (tetradecyltrimethylammonium chloride) is used as capture agent, phenethyl ester oil is used as foaming agent, and the pH is 2.0 to 3.0. Carry out 4 times of flotation to remove layered aluminosilicate mineral impurities such as kaolin, illite, pyrophyllite, etc., then wash with clean water until neutral, then dehydrate and dry for later use.
[0055] 2 High temperature activation and water q...
Embodiment 3
[0068] Take the 60-180 mesh quartz sand powder produced by a quartz sand factory in Heyuan City, Guangdong Province as an example
[0069] 1 Flotation: First flotation to remove feldspar impurities; then flotation to remove layered aluminosilicate mineral impurities
[0070] Using hydrofluoric acid and KOH as the pH regulator, dodecylamine as the capture agent, and No. 2 oil as the foaming agent, the quartz sand powder is flotation to remove feldspar mineral impurities under the condition of pH 2.0-3.0; then hydrochloric acid And sodium hydroxide as pH regulator, quaternary ammonium salt cation (tetradecyltrimethylammonium chloride) as capture agent, phenethyl ester oil as foaming agent, flotation under the condition of pH 2.0-3.0 Remove layered aluminosilicate mineral impurities such as kaolin, illite, pyrophyllite, etc., then wash with water until neutral, then dehydrate and dry for later use.
[0071] 2 High temperature alkali washing to remove impurities:
[0072] Put th...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com