A method of adding hydrophobically modified cuprous oxide to prepare anti-fouling and anti-corrosion coatings for fishing nets
A cuprous oxide and anti-corrosion coating technology, applied in anti-corrosion coatings, anti-fouling/underwater coatings, epoxy resin coatings, etc. performance, improved usability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] A method for adding hydrophobically modified cuprous oxide to prepare anti-fouling and anti-corrosion coatings for fishing nets, characterized in that it comprises the following steps:
[0024] (1) Irradiation modification of aluminum tripolyphosphate:
[0025] Pack 15 parts of aluminum tripolyphosphate into a polyethylene sealed bag, place it in a radiation field, and irradiate it with gamma rays whose total radiation dose is 100kGy;
[0026] (2) Modification of inorganic antifouling agent cuprous oxide:
[0027] Add 2 parts of modifying agent KH570 and 100 parts of distilled water to 10 parts of cuprous oxide, ultrasonically oscillate for 10 minutes, reflux at 80-82°C for 4 hours under magnetic stirring, filter under reduced pressure, and wash twice with absolute ethanol. Dry overnight in an oven at 50-53°C to obtain modified cuprous oxide;
[0028] (3) Anti-fouling and anti-corrosion coatings:
[0029] Add the graphene dispersion and carbon nanotubes oxidized and ...
Embodiment 2
[0036] A method for adding hydrophobically modified cuprous oxide to prepare anti-fouling and anti-corrosion coatings for fishing nets, characterized in that it comprises the following steps:
[0037] (1) Irradiation modification of aluminum tripolyphosphate:
[0038] Pack 25 parts of aluminum tripolyphosphate into a polyethylene sealed bag, place it in a radiation field, and irradiate it with gamma rays whose total radiation dose is 150kGy;
[0039] (2) Modification of inorganic antifouling agent cuprous oxide:
[0040] Add 4 parts of modifier KH570 and 150 parts of distilled water to 20 parts of cuprous oxide. After ultrasonic vibration for 15 minutes, reflux heating at 80-82°C for 5 hours with magnetic stirring reaction, vacuum filtration, and wash 3 times with absolute ethanol. Dry overnight in an oven at 50-53°C to obtain modified cuprous oxide;
[0041] (3) Anti-fouling and anti-corrosion coatings:
[0042] Add the graphene dispersion and carbon nanotubes modified by ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com