Acrylic fluid loss agents for oil well cement as well as preparation method and application of acrylic fluid loss agents
A technology of oil well cement and fluid loss reducer, which is applied in chemical instruments and methods, earthwork drilling and production, wellbore/well parts, etc. It can solve problems such as large fluctuations in raw material quality, poor high temperature resistance and salt resistance, and achieve Good cementing water loss reduction effect, strong high temperature resistance, and filtration loss reduction effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] This embodiment provides an acrylic fluid loss reducer for oil well cement, which consists of the following components in weight percentage:
[0041] Polymethacrylic acid, 15%;
[0044] The balance is triethanolamine.
[0045] Preparation method of acrylic fluid loss reducer for oil well cement: Take polymethacrylic acid and triethanolamine according to the ratio and put them into a mixing tank and stir for 15 minutes to make triethanolamine evenly cover polymethacrylic acid, then add calcium formate and sodium sulfate Stir for 25 minutes to complete the preparation of the fluid loss reducer.
Embodiment 2
[0047] This embodiment provides an acrylic fluid loss reducer for oil well cement, which consists of the following components in weight percentage:
[0048] Polyethylacrylate, 16%;
[0049] Calcium formate, 45%;
[0050] Sodium sulfate, 20%;
[0051] The balance is triethanolamine.
[0052] Preparation method of acrylic water loss reducer for oil well cement: Take polyethylacrylate and triethanolamine according to the ratio and put them into the mixing tank and stir for 16 minutes, so that the triethanolamine can evenly cover the polyacrylate, and then add calcium formate and sodium sulfate Stir for 27 minutes to complete the preparation of the fluid loss reducer.
Embodiment 3
[0054] This embodiment provides an acrylic fluid loss reducer for oil well cement, which consists of the following components in weight percentage:
[0055] Polyacrylamide, 17%;
[0056] Calcium formate, 46%;
[0057] Sodium sulfate, 25%;
[0058] The balance is triethanolamine.
[0059] Preparation method of acrylic fluid loss reducer for oil well cement: Take polyacrylamide and triethanolamine according to the ratio, put them into a mixing tank and stir for 17 minutes, so that triethanolamine can evenly cover polyacrylamide, then add calcium formate and sodium sulfate and stir for 30 minutes , to complete the preparation of the fluid loss reducer.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com