[0027] A production process of super waterproof leather, comprising the following steps:
[0028] (1) material selection: take the two-layer leather blank as raw material, weigh, put the two-layer leather blank into the drum, calculate the addition of other substances with the two-layer leather blank as 100 parts by mass, and the rotating speed of the drum is 5rad / min;
[0029] (2) Backwater: Add 200 parts by weight of water at 30°C and 0.5 parts by weight of formic acid into the drum, rotate for 50 minutes, and drain;
[0030] (3) Retanning: Add 140 parts by weight of water at 30° C. and 1 part by weight of dyestuff to the double-layer leather base after backwater, and rotate for 15 minutes, then add 1 part by weight of melamine retanning agent, and continue to rotate for 20 minutes. Then add 6 parts by weight of acrylic resin tanning agent, and rotate for 20 minutes; then add 0.5 parts by weight of waterproof oil, and rotate for 20 minutes; then add 1 part by weight of chr...
Embodiment 2
[0043] A production process of super waterproof leather, comprising the following steps:
[0044](1) material selection: take the two-layer leather blank as raw material, weigh, put the two-layer leather blank into the drum, calculate the addition of other substances with the two-layer leather blank as 100 parts by mass, and the rotating speed of the drum is 8rad / min;
[0045] (2) Backwater: add 250 parts by weight of water at 35°C and 0.6 parts by weight of formic acid into the drum, rotate for 60 minutes, and drain;
[0046] (3) Retanning: Add 150 parts by weight of water at 35°C and 1.5 parts by weight of dye to the double-layer leather base after returning to water, and rotate for 25 minutes, then add 2 parts by weight of dihydroamine compounding agent, and continue to rotate 30 minutes, then add 8 parts by weight of acrylic resin tanning agent, and rotate for 20 minutes; then add 1.2 parts by weight of waterproof oil, and rotate for 20 minutes; then add 2 parts by weigh...
Embodiment 3
[0059] A production process of super waterproof leather, comprising the following steps:
[0060] (1) Material selection: take the double-layer leather blank as raw material, weigh it, put the two-layer leather blank into the drum, calculate the addition of other substances with the double-layer leather blank as 100 parts by mass, and the rotating speed of the drum is 5~ 10rad / min;
[0061] (2) Backwater: add 300 parts by weight of water at 40°C and 0.7 parts by weight of formic acid into the drum, rotate for 70 minutes, and drain;
[0062] (3) Retanning: Add 160 parts by weight of 40°C water and 2 parts by weight of dye to the double-layer leather base after backwater, and rotate for 30 minutes, then add 3 parts by weight of melamine retanning agent, and continue to rotate for 40 minutes. Then add 10 parts by weight of acrylic resin tanning agent, and rotate for 25 minutes; then add 2 parts by weight of waterproof oil, and rotate for 25 minutes; then add 3 parts by weight of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com