Manufacturing method for lasting bacterium resisting and inhibiting type leather
A manufacturing method and leather technology, which can be applied in the fields of leather impregnation, leather surface treatment, small raw hide/large raw hide/leather/fur treatment, etc. Problems such as poor washing resistance, to achieve the effect of improving comprehensive utilization value, improving color saturation and fastness of dyeing, and lasting antibacterial properties
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] pre-tanning process
[0028] Pickling and pre-tanning: After 100Kg of goat alkali leather has been delimed and softened, add 80Kg of normal temperature water, add 8Kg of industrial salt, and rotate for 10 minutes; add 0.5Kg of formic acid (concentration 85%) diluted with 5Kg of water in advance, and rotate for 10 minutes; Add 0.4Kg sulfuric acid (98%) diluted with 8Kg water and rotate for 20 minutes; then add 0.4Kg sulfuric acid (98%) diluted with 8Kg water and rotate for 20 minutes; add 0.4Kg sulfuric acid (98%) diluted with 8Kg water and rotate 120 minutes; add 2Kg of oxidized N, N, N-trimethyl chitosan quaternary ammonium salt with an oxidation degree of 60%, and rotate for 90 minutes; stop the drum overnight, and rotate for 5 minutes every 120 minutes, before the end of pickling the next day Turn for 30 minutes;
[0029] Chrome tanning: Add 7Kg of chrome powder with an alkalinity of 33%, and rotate for 60 minutes; add 1Kg of sodium acetate, and rotate for 120 minut...
Embodiment 2
[0031] wet white process
[0032] Pre-tanning: 100Kg of oxalic leather is washed after softening and deliming, adding 100Kg of warm water at a temperature of 25°C, adding 4Kg of oxidized N-hydroxypropyltrimethylammonium chloride chitosan with an oxidation degree of 80%, and rotating for 180 minutes , let stand overnight;
[0033] Squeeze water: use a pass-through water squeezer to squeeze water, and the moisture content of the crust leather is required to be 50-55%;
[0034] Wrestling: Put the squeezed leather into the drum and rotate for 20 minutes;
[0035] Shave evenly: Shave evenly according to product requirements.
Embodiment 3
[0037] Retanning process
[0038] Retanning: 100Kg of wet blue leather, add 150Kg of water at a temperature of 35 to 40°C, add 3Kg of oxidized O-hydroxypropyltrimethylammonium chloride N-trimethyl chitosan with an oxidation degree of 30%, and rotate for 30 Minutes; add KMC chrome tanning powder 4Kg, Tannesco HN3Kg, and rotate for 90 minutes; dissolve 0.3Kg of baking soda in 5Kg of water, add to the drum in two times with an interval of 20 minutes; rotate for 40 minutes, stop the drum overnight.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com