Chitosan nano silver gel agent and uses thereof
A technology of chitosan nano and silver gel, which is applied in the direction of medical preparations containing no active ingredients, medical preparations containing active ingredients, inorganic active ingredients, etc., and can solve the problem that cannot be used for skin disease treatment and suppository restrictions. In order to achieve the effects of long duration of treatment, high moisture absorption and moisturizing effect, and excellent curative effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038]Embodiment 1: the preparation method of chitosan nano-silver gel
[0039] Self-made nano-silver, dispersed into a colloid with polyvinylpyrrolidone solution, the nano-silver content is 40000ppm,
[0040] Nano silver colloid: 5g.
[0041] Chitosan: 10g
[0042] Carbomer: 3g
[0043] Ethylene glycol: 2ml
[0044] Distilled water: 79g
[0045] Acetic acid: 1ml
[0046] The above-mentioned raw materials were placed in a stirrer and fully stirred to obtain a chitosan nano-silver gel with a nano-silver content of 2000 ppm and a chitosan concentration of 100 mg / g. After the preparation is completed, it is dispensed into gel dispensers or aluminum-plastic tubes.
[0047] The chitosan nano-silver gel prepared above can be used to treat female lower reproductive tract inflammation, cervicitis, cervical erosion, burn, scald, ulcer, bedsore infection or skin inflammation.
[0048] The specific usage and dosage for treating diseases such as cervicitis are as follows: figure 1...
Embodiment 2
[0050] The preparation method of embodiment 2 chitosan nano-silver gel
[0051] Homemade nano silver powder: 1mg
[0052] Chitosan: 60g
[0053] Glycerin: 2g
[0054] Carbomer: 3g
[0055] Distilled water: 32g
[0056] Acetic acid: 3ml
[0057] The above-mentioned raw materials were placed in a stirrer and fully stirred to obtain a chitosan nano-silver gel with a nano-silver content of 10 ppm and a chitosan concentration of 600 mg / g. After the preparation is completed, it is dispensed into gel dispensers or aluminum-plastic tubes.
[0058] Usage and dosage are the same as in Example 1.
Embodiment 3
[0059] The preparation method of embodiment 3 chitosan nano-silver gel
[0060] Homemade nano silver powder: 5g
[0061] Chitin: 1g
[0062] Polyethylene glycol: 3g
[0063] Distilled water: 91.5g
[0064] Phosphoric acid: 0.5ml
[0065] The above-mentioned raw materials were placed in a stirrer and stirred thoroughly to obtain a chitosan nano-silver gel with a nano-silver content of 50,000 ppm and a chitosan concentration of 10 mg / g. After the preparation is completed, it is dispensed into gel dispensers or aluminum-plastic tubes.
[0066] Usage and dosage are the same as in Example 1.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com