A dyeing method and fabric technology, applied in the field of dyeing pine needle fleece fabrics, can solve the problems of low color fastness, poor dyeing uniformity, and easy to produce color flowers of dyed fabrics, and achieve excellent color fastness to sunlight, dyeing Optimum effect, good dyeing uniformity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0039] The dyeing method of pine needle fleece fabric comprises the steps:
[0040] 1) Add 1 to 2 parts by weight of sodium silicate, 1.9 parts by weight of tea polyphenols, 2.8 parts by weight of hexyldecanol, 0.6 parts by weight of diethylenetriamine, and 45 parts by weight of vegetable dyes in turn into 150 parts by weight of deionized water, stir well, and heat to 55°C;
[0041] 2) Add 1.1 parts by weight of sodium persulfate, 0.5 parts by weight of sodium oleamide ethanesulfonate, 1.3 parts by weight of quaternized polyethyleneimine, and 1.9 parts by weight of dibutyl phthalate in turn, and continue stirring until fully Mix well and heat to 65°C;
[0042] 3) Soak the fabric in the dye vat for 30 minutes;
[0043] 4) drying the soaked fabric at 80°C;
[0044] 5) Soak the dried fabric in clean water and rinse for 30 minutes;
[0045] 6) Take out the rinsed fabric and let it dry naturally.
Embodiment 2
[0047] The dyeing method of pine needle fleece fabric comprises the steps:
[0048] 1) Add 1 weight part of sodium silicate, 1.9 weight part of tea polyphenols, 2.8 weight parts of hexyldecanol, 0.6 weight part of diethylenetriamine, and 45 weight parts of plant dyes into 150 weight parts of deionized water successively in the dye vat, Stir well and heat to 55°C;
[0049] 2) Add 1.1 parts by weight of sodium persulfate, 0.5 parts by weight of sodium oleamide ethanesulfonate, 1.3 parts by weight of quaternized polyethyleneimine, and 1.9 parts by weight of dibutyl phthalate in turn, and continue stirring until fully Mix well and heat to 65°C;
[0050] 3) Soak the fabric in the dye vat for 30 minutes;
[0051] 4) drying the soaked fabric at 80°C;
[0052] 5) Soak the dried fabric in clean water and rinse for 30 minutes;
[0053] 6) Take out the rinsed fabric and let it dry naturally.
Embodiment 3
[0055] The dyeing method of pine needle fleece fabric comprises the steps:
[0056] 1) Add 2 parts by weight of sodium silicate, 1.9 parts by weight of tea polyphenols, 2.8 parts by weight of hexyldecanol, 0.6 parts by weight of diethylenetriamine, and 45 parts by weight of vegetable dyes into 150 parts by weight of deionized water successively in the dye vat, Stir well and heat to 55°C;
[0057] 2) Add 1.1 parts by weight of sodium persulfate, 0.5 parts by weight of sodium oleamide ethanesulfonate, 1.3 parts by weight of quaternized polyethyleneimine, and 1.9 parts by weight of dibutyl phthalate in turn, and continue stirring until fully Mix well and heat to 65°C;
[0058] 3) Soak the fabric in the dye vat for 30 minutes;
[0059] 4) drying the soaked fabric at 80°C;
[0060] 5) Soak the dried fabric in clean water and rinse for 30 minutes;
[0061] 6) Take out the rinsed fabric and let it dry naturally.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com