Bituminous mixture used for thin layer overlay of cement concrete pavement and preparation and construction methods of bituminous mixture
A technology of asphalt mixture and cement concrete, which can be applied to cohesive pavements, roads, roads and other directions paved on site. It can solve the problems of high raw material requirements, achieve excellent performance, reduce pollution, and improve driving comfort and safety. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0030] (1) Components:
[0031] Aggregate: Basalt, the largest nominal particle size is 6.7mm, purchased from Jiangsu Xingyuan Mining Co., Ltd.;
[0032] Filler: Copper tailings powder, which can be selected from local or surrounding mines;
[0033] Among them, the weight ratio of aggregate to filler is 96%:4%. For the convenience of description, aggregate and filler are collectively referred to as "mineral material", and the gradation of mineral material is shown in Table 1.
[0034] Table 1 Mineral material gradation
[0035]
[0036] Asphalt: SBS polymer modified asphalt, the ratio of oil to stone is 5.8%, wherein the ratio of oil to stone is the ratio of the weight of asphalt to mineral aggregate. The asphalt was purchased from Jiangsu Baoli Asphalt Co., Ltd.
[0037] Fiber stabilizer: polyester fiber, the content of which is 0.2% of the weight of the mineral material, purchased from Changzhou Zhuwei Building Materials Co., Ltd.
[0038] Additives: It is made by mixing a compound syne...
Embodiment 2
[0056] (1) Components:
[0057] Aggregate: Limestone, the largest nominal particle size is 6.7mm, purchased from Jiangsu Xingyuan Mining Co., Ltd.;
[0058] Filler: Copper tailings powder, which can be selected from local or surrounding mines;
[0059] Among them, the weight ratio of aggregate to filler is 95%: 5%;
[0060] See Table 3 for mineral gradation
[0061] Table 3 Mineral material gradation
[0062]
[0063] Asphalt: Heavy traffic 70#A grade asphalt with a bitumen ratio of 6.1%, purchased from Jiangsu Zhongyou Xingneng Asphalt Co., Ltd.
[0064] Fiber stabilizer: lignin fiber, the content of which is 0.3% of the weight of the mineral material, purchased from Changzhou Zhuwei Building Materials Co., Ltd.
[0065] Additives: It is made by mixing a compound synergist and a warming agent, the former is 0.6% of the mass of the mineral aggregate, and the latter is 0.4% of the mineral aggregate. The compound synergist is purchased from Shanghai Honeywell Co., Ltd. The mixture was purch...
Embodiment 3
[0075] (1) Components:
[0076] Aggregate: Diabase, with a maximum nominal particle size of 6.7mm, purchased from Jiangsu Xingyuan Mining Co., Ltd.;
[0077] Filler: Copper tailings powder, which can be selected from local or surrounding mines;
[0078] Among them, the weight ratio of aggregate to filler is 96%: 4%;
[0079] See Table 5 for mineral gradation
[0080] Table 5 Mineral material grading
[0081]
[0082] Asphalt: SBS polymer modified bitumen bitumen with a bitumen ratio of 5.6%, purchased from Jiangsu Baoli Asphalt Co., Ltd.
[0083] Fiber stabilizer: polyester fiber, the content of which is 0.15% of the weight of the mineral material, purchased from Changzhou Zhuwei Building Materials Co., Ltd.
[0084] Additives: compound synergist, the mixing amount is 0.5% of the mass of the mineral material, the compound synergist is purchased from Shanghai Honeywell Co., Ltd. Here, no warming agent is used because the temperature is higher, and the asphalt mixture can be better paving a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com