Curing agent for sludge solidification and stabilization and preparation and application thereof
A technology of sludge solidification and solidifying agent, applied in chemical instruments and methods, fixed/solidified sludge treatment, water/sludge/sewage treatment, etc., can solve problems such as unsuitable site search, limited landfill capacity, and unsafety. , to achieve the effect of simplifying the treatment process and difficulty, shortening the maintenance period, and reducing the treatment cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0043] In this example, the solidification agent used for solidification and stabilization of the sludge in the sludge plant is mixed according to the following formula (percentage by weight):
[0044] Portland cement 20%,
[0045] Fly ash 30%,
[0046] Quicklime 30%,
[0048] Aluminum and calcium salts 5%,
[0049] Wherein, the aluminum salt is aluminum sulfate, the calcium salt is calcium chloride, and the mass ratio of aluminum sulfate to calcium chloride is 3:1.
[0050] Application of the above-mentioned curing agent: Add 500 kg of the above-mentioned curing agent to the original sludge with a moisture content as high as 96.3% per ton, and the strength can reach 143 kPa after 4 days, which meets the strength requirements of landfill disposal and construction fill. . After testing, the leachate concentration of heavy metals meets the identification standard of leaching toxicity.
Embodiment 2
[0052] In this example, the solidification agent used for solidification and stabilization of the sludge in the sludge plant is mixed according to the following formula (percentage by weight):
[0053] Portland cement 40%,
[0054] Fly Ash 10%,
[0055] Quicklime 30%,
[0057] Aluminum and calcium salts 5%,
[0058] Wherein, the aluminum salt is aluminum sulfate, the calcium salt is calcium chloride, and the mass ratio of aluminum sulfate to calcium chloride is 3:1.
[0059] Application of the above-mentioned curing agent: add 450kg of the above-mentioned curing agent to the raw sludge with a moisture content as high as 96.3% per ton, and the strength can reach 151kPa after 4 days, which meets the strength requirements of landfill disposal and construction fill. After testing, the leachate concentration of heavy metals meets the identification standard of leaching toxicity.
Embodiment 3
[0061]In this example, the solidification agent used for solidification and stabilization of the sludge in the sludge plant is mixed according to the following formula (percentage by weight):
[0062] Portland cement 40%,
[0063] Fly Ash 10%,
[0064] Quicklime: 10%,
[0065] Ferrous sulfate: 30%,
[0066] Aluminum and calcium salts: 10%,
[0067] Wherein, the aluminum salt is aluminum chloride, the calcium salt is calcium sulfate, and the mass ratio of aluminum chloride to calcium sulfate is 1:1.
[0068] Application of the above-mentioned curing agent: add 450 kg of the above-mentioned curing agent to the original sludge with a moisture content as high as 96.3% per ton, and the strength can reach 137kPa after 4 days, which meets the strength requirements of landfill disposal and construction fill. The concentration detection of the leach solution of heavy metals complied with the identification standard of leaching toxicity.
PUM
Property | Measurement | Unit |
---|---|---|
Strength | aaaaa | aaaaa |
Strength | aaaaa | aaaaa |
Strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com