An electrolysis device and a technology for inclusions, applied in the field of metallurgical engineering, can solve the problems of inability to meet production needs, the solution cannot meet the requirements, and the electrolysis time is long, and achieve the effects of improving electrolysis efficiency, increasing stirring effect, and accelerating electrolysis.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
example 1
[0049] In this embodiment, three groups of comparative experiments are set up by controlling the number of anodes.
[0050] In the test, the power supply voltage of the three groups of experiments was controlled to be 5V, the steel samples were not rotated, the central stirring was 4s / rotation, the temperature was controlled at about 0°C, and the electrolysis time was 12 hours. The only variable in the three sets of experiments was the number of anodes. The number of anodes is 1, 2 and 3 respectively and numbered 1, 2 and 3 respectively.
[0051] The following are the experimental results:
[0052]
[0053] It can be seen from the experimental results in the above table that the present invention can not only extract the inclusions in the steel sample, observe its complete three-dimensional structure and composition, but also greatly improve the electrolysis efficiency by adopting the method of parallel connection of anodes.
example 2
[0055] In this embodiment, three groups of experiments are set up by controlling the relationship between the anode rotation and the center rotation.
[0056] In the test, the power supply voltage of the three groups of experiments was controlled to be 5V, three anodes were connected in parallel, the central stirring was 4s / revolution, the temperature was controlled at about 0°C, and the electrolysis time was 12 hours. The only variable for the three sets of experiments was the anode rotation versus center rotation. They are normal center agitation without anode rotation, same direction anode rotation and center agitation, reverse anode rotation and center agitation, and are numbered 4, 5, and 6 in sequence.
[0057] If the rotation speed of the anode is 6s / revolution. The following are the experimental results:
[0058]
[0059] It can be seen from the experimental results in the above table that the present invention can not only extract the inclusions in the steel samp...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com