Novel color carbon treatment agent for leather and preparation method thereof
A treatment agent and leather technology, applied in fiber treatment, textile and papermaking, etc., can solve the problems of insufficient blackness, chroma, lack of metallic luster, and insufficient disposability, and achieve reasonable formula design, excellent product performance, Actionable effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0035] Add 18kg of toluene, 5kg of dimethylformamide, 12kg of ethyl acetate, 14kg of butyl acetate, and 4kg of nitrocellulose into the large tank in turn, stir and dissolve completely to obtain a transparent liquid.
[0036] Then add 1kg of fatty acid polyethylene glycol ester dispersant, 0.5kg of polyether siloxane leveling agent, 3kg of polyether modified polysiloxane, 20kg of soybean oil modified alkyd resin, and stir at a low speed. In some cases, add 2.5kg of silica matting powder, 15kg of high-pigment carbon black, and 5kg of color pigments. After adding all the materials, increase the rotation speed and disperse at a high speed for about 20 minutes at a stirring speed of 800-1000 rpm.
[0037] The stirred material is introduced into a vertical sand mill for grinding and dispersing evenly. After passing the inspection, it is packaged to obtain a new type of colored carbon treatment agent for leather.
Embodiment 2
[0039] Add 16kg of toluene, 5kg of dimethylformamide, 12kg of ethyl acetate, 10kg of butyl acetate, and 3kg of nitrocellulose into the large tank in turn, stir and dissolve completely to obtain a transparent liquid.
[0040] Then add 1kg of fatty acid polyethylene glycol ester dispersant, 0.5kg of polyether siloxane leveling agent, 2kg of polyether modified polysiloxane, 25kg of soybean oil modified alkyd resin, and stir at a low speed. In some cases, add 2.5kg of silica matting powder, 18kg of high-pigment carbon black, and 4kg of color pigments. After adding all the materials, increase the rotation speed and disperse at a high speed of 800-1000 rpm for about 20 minutes for later use.
[0041] The stirred material is introduced into a vertical sand mill for grinding and dispersing evenly. After passing the inspection, it is packaged to obtain a new type of colored carbon treatment agent for leather.
Embodiment 3
[0043] Add 15kg of toluene, 4kg of dimethylformamide, 10kg of ethyl acetate, 10kg of butyl acetate, and 2kg of nitrocellulose into a large tank in sequence, stir and dissolve completely to obtain a transparent liquid.
[0044] Add 1kg of fatty acid polyethylene glycol ester dispersant, 0.5kg of polyether siloxane leveling agent, 1.5kg of polyether modified polysiloxane, and 30kg of soybean oil modified alkyd resin in sequence and stir , Add 2kg of silica matting powder, 20kg of high-pigment carbon black, and 3kg of color pigment at low speed. After adding all the materials, increase the rotation speed and disperse at a high speed for about 20 minutes at a stirring speed of 800-1000 rpm.
[0045] The stirred material is introduced into a vertical sand mill for grinding and dispersing evenly. After passing the inspection, it is packaged to obtain a new type of colored carbon treatment agent for leather.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com