Writing board coated with surface-modified paint and writing liquid matched with writing board
A technology for surface modification and writing board, which is applied in the field of teaching utensils to achieve the effects of reducing writing cost, simple formula and simple production process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] The composition and content of the writing board paint are: 89.7 g of ethanol, 6 g of thymolphthalein, 1 g of acetone, 0.1 g of polyurethane, 0.2 g of xylene, 1 g of glutaraldehyde, and 2 g of polystyrene.
[0020] Preparation method of paint: Dissolve 6g of thymolphthalein in 89.7g of ethanol, add 1g of glutaraldehyde, react at 50°C for 1 hour, add 0.2g of xylene, 1g of acetone, 0.1g of polyurethane, stir evenly, Finally 2 g of polystyrene was added. Apply this paint to light-colored matt plastic panels and leave overnight to allow the paint to fully penetrate the pores.
[0021] Writing liquid formula: NaOH 9g, water 85.8mL, ethanol 5g, flavoring agent 0.2g.
[0022] Preparation method of writing liquid: Dissolve 9g NaOH in 85.8ml water, add 5g ethanol, then add 0.2g flavoring agent, stir well.
[0023] The blue handwriting is clear after writing. After the handwriting is dry, wipe it off with a damp cloth without handwriting residue and pollution. It can be reused ...
Embodiment 2
[0025] The composition and content of writing board paint are: ethanol 88g, thymolphthalein 5.4g, acetone 3.4g, polyurethane 0.2g, xylene 0.3g, glutaraldehyde 0.5g, polystyrene 2.1g
[0026] Preparation method of paint: Dissolve 5.4g thymolphthalein in 88g ethanol, add 0.5g glutaraldehyde, react at 40°C for 1.5 hours, add 0.3g xylene, 3.4g acetone, 0.2g polyurethane, stir Evenly, finally add 2.1g polystyrene. Apply this paint to light-colored matt plastic panels and leave overnight to allow the paint to fully penetrate the pores.
[0027] Writing liquid formula: NaOH 7g, water 86mL, ethanol 7g.
[0028] Preparation method of writing liquid: Dissolve 7g NaOH in 86ml water, add 7g ethanol, and stir well.
[0029] The blue handwriting is clear after writing. After the handwriting is dry, wipe it off with a damp cloth without handwriting residue and pollution. It can be reused for 7.5 months (10 hours a day).
Embodiment 3
[0031] The composition and content of writing board paint are: ethanol 85g, thymolphthalein 4.3g, acetone 3.6g, polyurethane 0.15g, xylene 0.25g, glutaraldehyde 2.7g, polyvinyl alcohol 4g
[0032] Preparation method of paint: dissolve 4.3g thymolphthalein in 85g ethanol, add 2.7g glutaraldehyde, react at 50°C for 1 hour, add 0.25g xylene, 3.6g acetone, add 0.15g polyurethane, Stir well, and finally add 4g of polyvinyl alcohol. Apply this paint to light matt panels and leave overnight to allow the paint to fully penetrate the pores.
[0033] Writing liquid formula: KOH 5.5g, water 87mL, ethanol 7g, fragrance 0.5g.
[0034] Preparation method of writing liquid: Dissolve 5.5g KOH in 87ml water, add 7g ethanol, then add 0.5g flavoring agent, stir well.
[0035] The blue handwriting is clear after writing. After the handwriting is dry, wipe it off with a damp cloth without handwriting residue and pollution. It can be reused for 6.8 months (10 hours a day).
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com