Eureka AIR delivers breakthrough ideas for toughest innovation challenges, trusted by R&D personnel around the world.

Aqueous dispersed alkyd blend colored paint and preparation method thereof

A dispersing and blending technology, used in the field of coatings, can solve the problems of slow drying and poor hardness of film formation, and achieve the effects of low volatile organic content, low odor and fast drying.

Active Publication Date: 2012-09-26
JIANGSU CHAMPION TECHNOLOGY GROUP CO LTD
View PDF4 Cites 16 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0012] The object of the present invention is to propose an economical and simple water-dispersible alkyd blending color paint in order to overcome the problems of slow film-forming and poor hardness after the solvent-based alkyd resin paint is added with a co-solvent.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Aqueous dispersed alkyd blend colored paint and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0037] First add 42kg of medium-oil alkyd resin (Jiangsu Champion Paint Industry Co., Ltd.) and 4 kg of mixed trimethylbenzene, start stirring (300 rpm), then add 6 kg of iron oxide yellow, 3.3 kg of medium chrome yellow, and 0.8 kg of rutile titanium dioxide , 5 kg superfine calcium carbonate, 5.5 kg precipitated barium sulfate, 0.35 kg BYK104S wetting agent, 0.5kg BYK141 defoamer, 0.6 kg 160 organobentonite and stir at an accelerated rate (900 rpm) for 15 minutes until evenly stirred (no powder on the edge of the pot) The material is attached, and there is no agglomeration in the pot);

[0038] Inhale the resulting mixture into a sand mill for sand grinding until the fineness is less than 35 microns;

[0039] Then start stirring (300 rpm) and add 5 kg C9 petroleum resin, 22 kg water-based additive (the water-based additive is the additive disclosed in Example 1 of the invention patent with the publication number CN 101230217A, Jiangsu Champion Paint Industry Co., Ltd.), 0.86...

Embodiment 2

[0042]First add 44kg of medium-oil alkyd resin (Jiangsu Champion Paint Industry Co., Ltd.) and 4 kg of 200# gasoline, start stirring (300 rpm), then add 0.64kg of phthalocyanine blue, 0.26kg of easily dispersible iron blue, and 3.5 kg of rutile Titanium dioxide, 6 kg ultra-fine calcium carbonate, 6.5 kg precipitated barium sulfate, 0.35 kg BYK104S wetting agent, 0.5 kg BYK052 defoamer, 0.6 kg 160 organic bentonite, accelerated stirring (900 rpm) for 15 min, until evenly stirred (pot edge No powder adhesion, no agglomeration in the pot);

[0043] Inhale the resulting mixture into a sand mill for sand grinding until the fineness is less than 35 microns;

[0044] Then start stirring (300 rpm) and add 5 kg C9 petroleum resin, 22.94 kg water-based additive (the water-based additive is the additive disclosed in Example 1 of the invention patent with the publication number CN 101230217A, Jiangsu Champion Paint Industry Co., Ltd.), 0.86 kgV-668 drier (Haimen Haifeng Chemical Auxiliar...

Embodiment 3

[0047] First add 46 kg of medium-oil alkyd resin (Jiangsu Champion Paint Industry Co., Ltd.) and 4kg of aromatic solvent oil S-1000#, start stirring (300 rpm), then add 4.74 kg of medium-pigment carbon black N234, 5.5 kg of ultra-fine carbonic acid Calcium, 6 kg of precipitated barium sulfate, 0.35 kg of BYK104S wetting agent, 0.5 kg of BYK052 defoamer, 0.6 kg of 160 organic bentonite, accelerated stirring (900 rpm) for 15 min, until evenly stirred (no powder adhered to the edge of the pot, no into agglomerates);

[0048] Inhale the resulting mixture into a sand mill for sand grinding until the fineness is less than 35 microns;

[0049] Then start stirring (300 rpm) and add 5 kg of C9 petroleum resin liquid, 22 kg of water-based additives (the water-based additives are the additives disclosed in Example 1 of the invention patent with the publication number CN 101230217A, Jiangsu Champion Paint Industry Co., Ltd.), 0.94 kg V-668 drier (Haifeng Chemical Auxiliary Co., Ltd., Hai...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses aqueous dispersed alkyd blend colored paint and a preparation method thereof. The aqueous dispersed alkyd blend colored paint is made of, by weight, 40%-46% of alkyd resin, 2%-6% of petroleum resin, 10%-28% of color filler, 0.3%-0.8% of defoaming agent, 0.4%-0.8% of organic clay, 0.3%-0.6% of wetting agent, 0.5%-1% of drier, 0.1%-0.3% of anti-skinning agent, 20%-35% of cosolvent and 5%-10% of organic solvent. The aqueous dispersed alkyd blend colored paint is fresh and natural in smell and has excellent gloss, bonding force, flexibility, water resistance, corrosion resistance and outdoor durability.

Description

technical field [0001] The invention relates to the field of coatings, in particular to a water-dispersible alkyd blend paint and a preparation method thereof. Background technique [0002] Alkyd resin is the most important resin for coatings, and it is also the largest and earliest synthetic resin used in the coatings industry. Most of the alkyd resins currently on trial are solvent-based resins, which are the main source of volatile organic compounds (VOC). With the gradual improvement of people's environmental requirements, countries have put forward strict restrictions on the content of VOC in coatings. Since water is non-toxic, odorless, non-flammable and cheap, introducing water into the paint can not only reduce the production cost, but also greatly reduce the VOC content. [0003] There are currently three methods of introducing water into an alkyd paint to form a dispersion: [0004] 1. Make the traditional alkyd resin contain excessive carboxyl groups, and neutr...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C09D167/08C09D157/02C09D7/12
Inventor 谢海张波张秋杰郑磊
Owner JIANGSU CHAMPION TECHNOLOGY GROUP CO LTD
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Eureka Blog
Learn More
PatSnap group products