Preparation of polymer composite gelling agent for grouting and application method thereof
A composite glue and polymer technology, applied in the field of gelling agent, can solve problems such as complex process, low gel strength, easy to collapse pulp, etc., and achieve good application prospects, wide application and wide performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] (A) Composite gelling agent
[0033] According to weight percentage, weigh 20% bentonite, 20% calcium sulfate, 10% calcium hydroxide, 12% vegetable gum, 12% carboxymethyl cellulose, 16% polyacrylamide, 8% carbonic acid Sodium hydrogen, 0.6% sodium hydroxide, and 1.4% ferric chloride were uniformly mixed to prepare a gelling agent.
[0034] (B) slurry preparation (according to parts by mass)
[0035] (1) The loess is sieved into powders with a particle size less than 8mm, and 500 parts of soil and 400 parts of water are evenly mixed into a slurry;
[0036] (2) take 1 part of gelling agent again;
[0037] (3) The gelling agent weighed is added into 100 parts of water and uniformly mixed into an aqueous gelling agent solution;
[0038] (4) Inject the mixed gelling agent aqueous solution into the mud-water slurry under a certain pressure.
[0039] (5) The muddy water slurry injected with the gelling agent aqueous solution is further mixed and stirred, and gel is formed ...
Embodiment 2
[0041] (A) Composite gelling agent
[0042] According to weight percentage, weigh 22% bentonite, 18% calcium sulfate, 5% calcium hydroxide, 20% vegetable gum, 20% carboxymethyl cellulose, 8% polyacrylamide, 5% carbonic acid Sodium hydrogen, 1% sodium hydroxide, and 1% ferric chloride are uniformly mixed to prepare a gelling agent.
[0043] (B) slurry preparation (according to parts by mass)
[0044] (1) The loess is sieved into a powder with a particle size less than 8mm, and 500 parts of soil and 400 parts of water are evenly mixed into a slurry;
[0045] (2) take 5 parts of composite gelling agent again;
[0046] (3) The gelling agent weighed is added into 100 parts of water and uniformly mixed into an aqueous gelling agent solution;
[0047] (4) Inject the mixed gelling agent aqueous solution into the mud-water slurry;
[0048] (5) The mud-water slurry injected with the gelling agent aqueous solution is further mixed and stirred for 6 minutes to form a gel, and simultan...
Embodiment 3
[0050] (A) Composite gelling agent
[0051] According to the percentage by weight, weigh 18% bentonite, 16% calcium sulfate, 15% calcium hydroxide, 10% vegetable gum, 12% carboxymethyl cellulose, 16% polyacrylamide, 10% carbonic acid Sodium hydrogen, 1% sodium hydroxide, and 2% ferric chloride were uniformly mixed to prepare a gelling agent.
[0052] (B) slurry preparation (according to parts by mass)
[0053] (1) The loess is sieved into a powder with a particle size less than 8mm, and 550 parts of soil and 350 parts of water are evenly mixed into a slurry;
[0054] (2) take 2 parts of gelling agent again;
[0055] (3) The gelling agent weighed is added into 100 parts of water and uniformly mixed into an aqueous gelling agent solution;
[0056] (4) Add the mixed gelling agent aqueous solution into the mud-water slurry.
[0057] (5) The mud-water slurry injected with the gelling agent aqueous solution is further mixed and stirred for 5 minutes to form an accumulative mud c...
PUM
Property | Measurement | Unit |
---|---|---|
Granularity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com