Synthetic method of acrylamide selective adsorption functional material
A technology of functional materials and acrylamide, applied in chemical instruments and methods, other chemical processes, etc., can solve the problem of false positive results and high test results, and achieve the effects of easy control of reaction conditions, scientific process, and strong resistance to harsh environments
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] The steps of a synthetic method of acrylamide selective adsorption functional material:
[0021] 1) Add 10 ml of N,N-dimethylformamide, 0.243 g of propionamide, 2.293 g of methacrylic acid, and 26.4 g of ethylene glycol dimethacrylate into a 100 ml stoppered Erlenmeyer flask, and mix for 15 minutes by ultrasonic , standing at room temperature for 12 hours to carry out pre-polymerization.
[0022] 2) Add 0.264 g of azobisisobutyronitrile to the above solution, fill it with nitrogen for 15 minutes, transfer it to an ampoule bottle and seal the tube, and then put it in a 60°C water bath to initiate polymerization for 20 hours. The resulting bulk product is the precursor of the imprinted polymer material.
[0023] 3) The above-mentioned polymer was pulverized, placed in a vacuum drying oven at 100° C. for 10 hours, and passed through a 250-mesh sieve. Add methanol to the polymer particles, ultrasonically clean for 2 hours, shake on an oscillator for 8 hours, filter, wash ...
Embodiment 2
[0025] The steps of a synthetic method of acrylamide selective adsorption functional material:
[0026] 1) Add 10 ml of N,N-dimethylformamide, 0.243 g of propionamide, 2.293 g of methacrylic acid, and 26.4 g of ethylene glycol dimethacrylate into a 100 ml stoppered Erlenmeyer flask, and mix for 10 minutes by ultrasonic , standing at room temperature for 8 hours to carry out pre-polymerization.
[0027] 2) Add 0.264 g of azobisisobutyronitrile to the above solution, fill with nitrogen gas for 10 minutes, transfer to an ampoule to seal the tube, and then put it in a water bath at 55° C. to initiate polymerization for 20 hours. The resulting bulk product is the precursor of the imprinted polymer material.
[0028] 3) The above-mentioned polymer was pulverized, placed in a vacuum drying oven at 100° C. for 15 hours, and passed through a 250-mesh sieve. Add methanol to the polymer particles, ultrasonically clean for 4 hours, shake on an oscillator for 10 hours, filter, wash with ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com