Modifying reclaiming formulation for engineering plastic
A technology for engineering plastics and modification, applied in the field of plastic modification treatment, can solve problems such as uneconomical environment, pollution, corrosion of molding equipment and molds, and achieve good economic and social benefits.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0054] First, take PC / ABS secondary materials, PC secondary materials, compatibilizers, toughening agents, brominated small molecule flame retardants, antimony-based flame retardants, antioxidants, ultraviolet absorbers and other components, in parts by weight The following composition formula blends all raw materials:
[0055] PC / ABS secondary material 81;
[0056] PC secondary material 5;
[0057] SMA2;
[0058] MBS 5;
[0059] Decabromodiphenylethane 5;
[0060] Sb 2 o 3 2;
[0061] Antioxidant 0.3;
[0062]UV absorber 0.3.
[0063] Secondly, the above-mentioned blend is mixed and granulated in an extruder;
[0064] Thirdly, the obtained kneading and granulation can be processed into a finished product after modification of the secondary material through injection molding.
[0065] The performance test of the modified finished product is compared with the performance of the PC / ABS raw material alloy. The test comparison results are sho...
Embodiment 2
[0070] First, take PC / ABS secondary materials, PC secondary materials, compatibilizers, toughening agents, brominated small molecule flame retardants, antimony-based flame retardants, antioxidants, ultraviolet absorbers and other components, in parts by weight The following composition formula blends all raw materials:
[0071] PC / ABS secondary material 75;
[0072] PC secondary material 8;
[0073] SMA2;
[0074] MBS 5;
[0075] Decabromodiphenylethane 7;
[0076] Sb 2 o 3 3;
[0077] Antioxidant 0.2;
[0078] UV absorber 0.2.
[0079] Secondly, the above-mentioned blend is mixed and granulated in an extruder;
[0080] Thirdly, the obtained kneading and granulation can be processed into a finished product after modification of the secondary material through injection molding.
[0081] The performance test of the modified finished product is compared with the performance of the PC / ABS raw material alloy. The test comparison results are sh...
Embodiment 3
[0085] First, take PC / ABS secondary materials, PC secondary materials, compatibilizers, toughening agents, brominated small molecule flame retardants, antimony-based flame retardants, antioxidants, ultraviolet absorbers and other components, in parts by weight The following composition formula blends all raw materials:
[0086] PC / ABS secondary material 69;
[0087] PC secondary material 12;
[0088] SMA4;
[0089] MBS 3;
[0090] Decabromodiphenylethane 9;
[0091] Sb 2 o 3 3;
[0092] Antioxidant 0.1;
[0093] UV absorber 0.1.
[0094] Secondly, the above-mentioned blend is mixed and granulated in an extruder;
[0095] Thirdly, the obtained kneading and granulation can be processed into a finished product after modification of the secondary material through injection molding.
[0096] The performance test of the modified finished product is compared with the performance of the PC / ABS raw material alloy. The test comparison results are sho...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com