Construction method by utilizing solidified earth from sludge
A construction method and soil solidification technology, which is applied in solid waste management, dehydration/drying/concentrated sludge treatment, sustainable waste treatment, etc., can solve the problems of occupying large cultivated land and polluting the environment, so as to save cultivated land, avoid pollution, The effect of solving difficult problems
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] First dig out the silt from Taihu Lake (or other rivers, lakes and seas), and remove the lumps and sticks;
[0018] Afterwards, the sludge that does not contain lumps and sticks is piled up together, and the weight percentage of its water content is 40% and close to the liquid limit by natural precipitation and evaporation of moisture.
[0019] Afterwards, put the silt with a water content of 40% and close to the liquid limit into the agitator, add cement and fly ash, stir for 30 to 80 seconds, and mix evenly to obtain solidified silt soil; wherein: In the cubic meter of sludge, the addition of cement is 50kg, and the addition of fly ash is 50kg;
[0020] Afterwards, pile the solidified silt for 2 to 3 days to allow it to continue to solidify. When it has early strength and is ready for mechanical paving, it can be laid in layers on the subgrade.
[0021] After paving each layer of solidified silt soil, use 5 tons of sheep foot roller to roll it 6 to 8 times for compa...
Embodiment 2
[0026] First dig out the silt from Taihu Lake (or other rivers, lakes and seas), and remove the lumps and sticks;
[0027] Afterwards, the sludge that does not contain lumps and sticks is piled together, and the weight percentage of its water content is 50% and close to the liquid limit through natural precipitation and evaporation of moisture.
[0028] Afterwards, put the silt with a water content of 50% and close to the liquid limit into the agitator, add cement and fly ash, stir for 30 to 80 seconds, and mix uniformly to obtain solidified silt soil; wherein: In the cubic meter of sludge, the addition of cement is 75kg, and the addition of fly ash is 95kg;
[0029] Afterwards, pile the solidified silt for 2 to 3 days to allow it to continue to solidify. When it has early strength and is ready for mechanical paving, it can be laid in layers on the embankment.
[0030] After paving each layer of solidified silt soil, use 5 tons of sheep foot roller to roll it 6 to 8 times fo...
Embodiment 3
[0035] First dig out the silt from Taihu Lake (or other rivers, lakes and seas), and remove the lumps and sticks;
[0036] Afterwards, the sludge that does not contain lumps and sticks is piled together, and the weight percentage of its water content is 60% and close to the liquid limit by natural precipitation and evaporation of moisture.
[0037] Afterwards, put the silt with water content of 60% and close to the liquid limit into the mixer, add cement and fly ash, stir for 30 to 80 seconds, and mix evenly to obtain solidified silt soil; wherein: In the cubic meter of sludge, the addition of cement is 100kg, and the addition of fly ash is 150kg;
[0038] Afterwards, pile the solidified silt for 2 to 3 days to allow it to continue to solidify. When it has early strength and can be paved mechanically, it can be paved in layers on low-lying ground;
[0039] After paving each layer of solidified silt soil, use 5 tons of sheep foot roller to roll it 6 to 8 times for compaction ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com