Preparation process of flame-retardant embroidery
A technology of preparation technology and flame retardancy, which is applied in the field of preparation technology of embroidery products, can solve the problems of poor flame resistance, hidden safety hazards, and easy burning of embroidery products, and achieve anti-static, safety, and durability The effect of grinding performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A preparation process for flame-retardant embroidery, comprising the following steps:
[0023] Step 1: Blend the modified nylon fiber, flame-retardant viscose fiber and aramid fiber into a single yarn according to the weight ratio of 1:5:4, and then twist the two single yarns according to the twist direction of Z / S to form a Yarn, the warp density of the warp is set to 370 / 10cm, the weft density of the weft is set to 260 / 10cm, a 3 / 1 twill weave is used, and the machine weaves according to 95% fabric tightness to obtain flame retardant embroidery fabric;
[0024] Step 2: Pretreat the embroidery base fabric with a silane coupling agent solution for 10 minutes, and then dry it at 40°C for 10 minutes;
[0025] Step 3: Print the embroidery pattern on the embroidery base cloth, place the embroidery base cloth on the embroidery machine, the embroidery machine will embroider according to the pre-designed pattern, and then sew the embroidery embroidery, check whether the embroi...
Embodiment 2
[0034] A preparation process for flame-retardant embroidery, comprising the following steps:
[0035] Step 1: Blend the modified nylon fiber, flame-retardant viscose fiber and aramid fiber into a single yarn according to the weight ratio of 1:5:4, and then twist the two single yarns according to the twist direction of Z / S to form a Yarn, the warp density of the warp is set to 380 / 10cm, the weft density of the weft is set to 270 / 10cm, a 3 / 1 twill weave is used, and the weaving is carried out on the machine according to 95% fabric tightness to obtain flame retardant embroidery fabric;
[0036] Step 2: Pretreat the embroidery base fabric with a silane coupling agent solution for 13 minutes, and then dry it at 50°C for 20 minutes;
[0037] Step 3: Print the embroidery pattern on the embroidery base cloth, place the embroidery base cloth on the embroidery machine, the embroidery machine will embroider according to the pre-designed pattern, and then sew the embroidery embroidery, c...
Embodiment 3
[0046] A preparation process for flame-retardant embroidery, comprising the following steps:
[0047] Step 1: Blend the modified nylon fiber, flame-retardant viscose fiber and aramid fiber into a single yarn according to the weight ratio of 1:5:4, and then twist the two single yarns according to the twist direction of Z / S to form a Yarn, the warp density of the warp is set to 390 / 10cm, the weft density of the weft is set to 280 / 10cm, a 3 / 1 twill weave is used, and the weaving is carried out on the machine according to 95% fabric tightness to obtain flame retardant embroidery fabric;
[0048] Step 2: Pretreat the embroidery base cloth with a silane coupling agent solution for 15 minutes, and then dry it at 60°C for 30 minutes;
[0049] Step 3: Print the embroidery pattern on the embroidery base cloth, place the embroidery base cloth on the embroidery machine, the embroidery machine will embroider according to the pre-designed pattern, and then sew the embroidery embroidery, ch...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com