A mass fraction, corrosion inhibitor technology, applied in chemical instruments and methods, earthwork drilling, drilling composition, etc., can solve problems such as disappearance, corrosion rate increase, easy coking, etc., to reduce steric hindrance effect, improve Conversion rate, effect of adsorption film densification
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0037] A corrosion inhibitor suitable for a hydrochloric acid system with a mass fraction of 20-28% and an ambient temperature of 90°C, the composition of which is calculated by weight percentage:
[0038] Quinoline quaternary ammonium salt: 14%;
[0039] Imidazoline quaternary ammonium salt: 14%;
[0040] Alkynol: 8%;
[0041] Acid-soluble metal salts: 3%, specifically copper chloride dihydrate;
[0042] Low molecular organic acid: 5%, specifically formic acid;
[0043] Surfactant: 1%, specifically OP-10 (polyoxyethylene octylphenol ether-10);
[0044] Organic solvent: 45%, specifically methanol;
[0045] Deionized water: 10%.
[0046] A corrosion inhibitor suitable for a hydrochloric acid system with a mass fraction of 20-28% and an ambient temperature of 90°C, the preparation method of which is as follows:
[0047] (1) Synthesis of quinoline quaternary ammonium salt:
[0048] First, the raw materials are selected by weight percentage as follows: quinoline: 39.4%; ben...
Embodiment 2
[0058] A corrosion inhibitor suitable for a hydrochloric acid system with a mass fraction of 20-28% and an ambient temperature of 120°C, the composition of which is calculated by weight percentage:
[0059] Quinoline quaternary ammonium salt: 18%;
[0060] Imidazoline quaternary ammonium salt: 18%;
[0061] Alkynol: 10%;
[0062] Acid-soluble metal salt: 5%, specifically cuprous bromide;
[0063] Low molecular organic acid: 8%, specifically a mixture of formic acid and oxalic acid, the mass ratio of the two is 2:1;
[0064] Surfactant: 2%, specifically OP series surfactants, OP-10 is still selected in this embodiment;
[0065] Organic solvent: 31%, specifically DMF (N,N-dimethylformamide);
[0066] Deionized water: 8%.
[0067] A corrosion inhibitor suitable for a hydrochloric acid system with a mass fraction of 28% and an ambient temperature of 120°C. Its preparation method is as follows:
[0068] (1) Synthesis of quinoline quaternary ammonium salt:
[0069] First, the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com