Method for purifying manganese sulfate in magnesium-rich manganese sulfate solution
A technology of magnesium-rich manganese sulfate solution and magnesium-rich manganese sulfate, applied in the direction of manganese sulfate, etc., to achieve the effect of simple process and low production cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] First prepare the magnesium-rich manganese sulfate solution, and measure the Mn 2+ Concentration: 90g / L, Mg 2+ The concentration is 70g / L, Ca 2+ The concentration is 0.3g / L. Heat the above-mentioned magnesium-rich manganese sulfate solution at a temperature of 160°C to carry out the first high-temperature crystallization, and stir at a stirring speed of 30r / min to obtain a system after the primary crystallization, and carry out the system after the primary crystallization at a temperature of 155°C Filter to obtain crystals after primary crystallization.
[0034] Dissolve the crystals after primary crystallization in water to obtain the dissolved system, and measure the Mn 2+ The concentration is: 78g / L, Mg 2 + The concentration is 21g / L, and the dissolved system is heated at 140°C for the second high-temperature crystallization, and stirred at a stirring speed of 30r / min to obtain the secondary crystallized system, and the secondary crystallized system is obtained ...
Embodiment 2
[0036] The difference between embodiment 2 and embodiment 1 is that in the magnesium-rich manganese sulfate solution, Mn 2+ Concentration: 80g / L, Mg 2+ The concentration is 80g / L, Ca 2+ The concentration is 0.1g / L, and the mass ratio of manganese to magnesium in crystals after secondary crystallization is calculated to be 9.87.
Embodiment 3
[0038] The difference between embodiment 3 and embodiment 1 is that in the magnesium-rich manganese sulfate solution, Mn 2+ Concentration: 130g / L, Mg 2+ The concentration is 50g / L, Ca 2+ The concentration is 0.5g / L, and the mass ratio of manganese to magnesium in crystals after secondary crystallization is calculated to be 15.78.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com