Aqueous woodware solid color paint and preparation method thereof
A wood and solid color technology, applied in the field of coatings, can solve the problems of affecting the appearance of wood products, peeling, paint film falling off, etc., and achieve the effect of compact combination, less film-forming additives and good adhesion
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] A water-based solid color paint for woodware, comprising the following raw material components, the weight ratio of each component raw material is:
[0037] Pure water 3.00%
[0038] Pigment conditioner 1.50%
[0039] Filler 20.00%
[0040] Emulsion A 70.00%
[0041] Coalescing agent 4.00%
[0042] Substrate wetting agent 0.50%
[0043] Defoamer 0.50%
[0044] Rheology modifier 0.50%.
[0045] The preparation method of above-mentioned water-based solid color paint for woodware, comprises the following steps:
[0046] A. Select an electronic scale with an accuracy of 0.01g to weigh raw materials such as pure water, pigment modifier, filler, emulsion A, film-forming aid, substrate wetting agent, defoamer, and rheological additive according to the proportion, and place them in categories;
[0047] B. Add pure water, pigment modifier and filler in order in the sand mill dispersing multi-purpose machine, stir and disperse at a speed of 1000-1200 rpm for 1-2 hours unti...
Embodiment 2
[0051] A water-based solid color paint for woodware, comprising the following raw material components, the weight ratio of each component raw material is:
[0052] Pure water 5.00%
[0053] Pigment conditioner 2.50%
[0054] Filler 25.00%
[0055] Emulsion A 60.00%
[0056] Coalescing aid 5.00%
[0057] Substrate wetting agent 0.50%
[0058] Defoamer 0.50%
[0059] Rheology modifier 0.50%.
[0060] The preparation method of above-mentioned water-based solid color paint for woodware, comprises the following steps:
[0061] A. Select an electronic scale with an accuracy of 0.01g to weigh raw materials such as pure water, pigment modifier, filler, emulsion A, film-forming aid, substrate wetting agent, defoamer and rheological additive according to the proportion, and place them in categories;
[0062] B. Add pure water, pigment modifier and filler in order in the sand mill dispersing multi-purpose machine, stir and disperse at a speed of 1000-1200 rpm for 1-2 hours until u...
Embodiment 3
[0066] A water-based solid color paint for woodware, comprising the following raw material components, the weight ratio of each component raw material is:
[0067] Pure water 10.00%
[0068] Pigment conditioner 3.00%
[0069] Filler 25.00%
[0070] Emulsion A 55.00%
[0071] Coalescing agent 6.00%
[0072] Substrate wetting agent 0.20%
[0073] Defoamer 0.30%
[0074] Rheology modifier 0.50%.
[0075] The preparation method of above-mentioned water-based solid color paint for woodware, comprises the following steps:
[0076] A. Select an electronic scale with an accuracy of 0.01g to weigh raw materials such as pure water, pigment modifier, filler, emulsion A, film-forming aid, substrate wetting agent, defoamer, and rheological additive according to the proportion, and place them in categories;
[0077] B. Add pure water, pigment regulator and filler in order in the sand mill dispersing multi-purpose machine, stir and disperse at a speed of 1000-1200 rpm for 1-2 hours unti...
PUM
Property | Measurement | Unit |
---|---|---|
tack-free time | aaaaa | aaaaa |
hardness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com