Embodiment 1
[0035] A method for preparing a silicon-coated composite material based on porous carbon, comprising the steps of:
[0036] Step 1, adding phenolic resin to absolute ethanol, stirring until completely dissolved, then adding polyvinylpyrrolidone and stirring until completely dissolved, to obtain a mixed dispersion;
[0037] Step 2, adding the aluminum chloride solution to the mixed dispersion liquid and ultrasonically reacting for 10 minutes, and then pouring concentrated ammonia water until no precipitation occurs to obtain a mixed suspension;
[0038] Step 3, adding the mixed suspension into the reaction kettle for ultrasonic reaction for 1 h, then adding it into the vacuum distillation kettle and reacting until completely evaporated to dryness to obtain a mixed solid;
[0039] Step 4, adding the mixed solid into the reaction kettle, sealing it for anaerobic carbonation for 3 hours, taking it out, soaking it in hydrochloric acid solution for 30 minutes, removing and drying to...
Embodiment 2
[0051] A method for preparing a silicon-coated composite material based on porous carbon, comprising the steps of:
[0052]Step 1, adding phenolic resin to absolute ethanol, stirring until completely dissolved, then adding polyvinylpyrrolidone and stirring until completely dissolved, to obtain a mixed dispersion;
[0053] Step 2, adding the aluminum chloride solution to the mixed dispersion liquid for ultrasonic reaction for 20 minutes, and then pouring concentrated ammonia water until no precipitation occurs, to obtain a mixed suspension;
[0054] Step 3, adding the mixed suspension into the reaction kettle for ultrasonic reaction for 3 hours, then adding it into the vacuum distillation kettle and reacting until completely evaporated to dryness to obtain a mixed solid;
[0055] Step 4, adding the mixed solids into the reaction kettle and sealing them for anaerobic carbonation for 8 hours, taking them out, soaking them in hydrochloric acid solution for 60 minutes, removing and...
Embodiment 3
[0067] A method for preparing a silicon-coated composite material based on porous carbon, comprising the steps of:
[0068] Step 1, adding phenolic resin to absolute ethanol, stirring until completely dissolved, then adding polyvinylpyrrolidone and stirring until completely dissolved, to obtain a mixed dispersion;
[0069] Step 2, adding the aluminum chloride solution to the mixed dispersion liquid and ultrasonically reacting for 15 minutes, and then pouring concentrated ammonia water until no precipitation occurs to obtain a mixed suspension;
[0070] Step 3, adding the mixed suspension into the reaction kettle for ultrasonic reaction for 2 hours, then adding it into the vacuum distillation kettle and reacting until completely evaporated to dryness to obtain a mixed solid;
[0071] Step 4, adding the mixed solid into the reaction kettle, sealing it for anaerobic carbonation for 6 hours, taking it out, soaking it in hydrochloric acid solution for 50 minutes, removing and dryin...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com