A leather and pearlescent technology, which is applied in the field of iridescent pearlescent leather and its preparation, can solve the problems of difficult leather surface brightness, the beauty of the leather surface does not play a big role, etc., and achieves the improvement of fluency, transparency and visual effect. Effect

Active Publication Date: 2021-04-06
漳州香洲皮革有限公司
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Although this process can effectively improve the brightness of the leather, it is difficult to maintain the brightness of the leather surface for a long time, and at the same time, it does not have much effect on the appearance of the leather surface.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Iridescent pearlescent leather and preparation method thereof
  • Iridescent pearlescent leather and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0035] Iridescent pearl leather, including leather and coating, said coating includes the following components in terms of leather mass percentage: 7% of the first coating, 12% of the second coating and 12% of the third coating, wherein, The third coating, the second coating and the first coating are sequentially attached to the leather.

[0036] The first coating comprises the following components in terms of leather mass percentage: 6% maleic anhydride, 7% sodium sulfite, 8% sodium 2-hydroxyethanesulfonate, and 9% butanone;

[0037] The second coating comprises the following components in terms of leather mass percentage: 2% toner, 13% polyvinyl acetate; the toner is iridescent color powder.

[0038] The third coating includes the following components in terms of leather weight percentage: 0.7% of pearl powder, 8% of polyacrylamide, and 3% of polymethyl methacrylate.

[0039] The preparation method of described iridescent pearl leather, comprises the steps:

[0040] Step 1...

Embodiment 2

[0056] Iridescent pearl leather, including leather and coating, said coating includes the following components in terms of leather mass percentage: 8% of the first coating, 14% of the second coating and 14% of the third coating, wherein, The third coating, the second coating and the first coating are sequentially attached to the leather.

[0057] The first coating comprises the following components in terms of leather mass percentage: 8% maleic anhydride, 8% sodium sulfite, 9% sodium 2-hydroxyethanesulfonate, and 11% methyl ethyl ketone;

[0058] The second coating comprises the following components in terms of leather mass percentage: 3% toner, 14% polyvinyl acetate; the toner is iridescent color powder.

[0059] The third coating layer includes the following components according to the weight percentage of leather: pearl powder 0.8%, polyacrylamide 9%, polymethyl methacrylate 5%.

[0060] The preparation method of described iridescent pearly leather comprises the steps:

[0...

Embodiment 3

[0077] Iridescent pearlescent leather, comprising leather and a coating, the coating comprising the following components in terms of the mass percentage of leather: 10% of the first coating, 15% of the second coating and 15% of the third coating, wherein, The third coating, the second coating and the first coating are sequentially attached to the leather.

[0078] The first coating layer comprises the following components according to the mass percentage of leather: maleic anhydride 10%, sodium sulfite 9%, sodium 2-hydroxyethane sulfonate 11%, butanone 13%;

[0079] The second coating layer includes the following components in terms of mass percentage of leather: 3% toner, 16% polyvinyl acetate; the toner is iridescent toner.

[0080] The third coating layer comprises the following components according to the weight percentage of leather: pearl powder 1.0%, polyacrylamide 9%, polymethyl methacrylate 6%.

[0081] The preparation method of described iridescent pearly leather co...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
tensile strengthaaaaaaaaaa
Login to View More

Abstract

The invention discloses an iridescent pearlescent leather and a preparation method thereof, belonging to the technical field of leather. The iridescent pearlescent leather of the present invention comprises leather and a coating, and the coating comprises the following components in terms of the mass percentage of the leather: 7-10% of the first coating, 12-15% of the second coating and 12-15% of the third coating 12-15% of the layer, wherein, the third coating, the second coating and the first coating are sequentially coated on the leather. The preparation method of the iridescent pearlescent leather includes the following steps: preparing the coating Material, coating coating material and drying, the surface of the obtained iridescent pearlescent leather has a reflective effect, the tensile strength is as high as 31 MPa in the transverse direction, 33 MPa in the longitudinal direction, and the friction fading reaches level 4. It has strong friction resistance and yellowing resistance. powerful.

Description

technical field [0001] The invention belongs to the technical field of leather, and in particular relates to an iridescent pearlescent leather and a preparation method thereof. Background technique [0002] With the development of society, more and more high-tech products come out, and many advanced products have a glamorous appearance. Leather products are favored by people for their durability. The surface of traditional leather products is wear-resistant and does not fade. However, if the leather surface is made to have a crystal light effect, it is easy to reduce the wear resistance of the leather. [0003] The Chinese invention patent application with the application number 201510782629.0 discloses a leather high-brightness treatment process, which includes the following steps: soak the leather in 5-15% salt water at 30-40°C for 20-40 minutes, and put the leather in the transfer tank after removal. In the drum, add leather brightener at 30-40°C, turn multi-function at ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C14C11/00C09D131/04C09D133/26C09D133/12C09D7/61
CPCC09D131/04C09D133/26C14C11/003C09D7/61C08L33/12
Inventor 许维奇林汉彬陈启明
Owner 漳州香洲皮革有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products