Jun porcelain jade glaze and preparation method thereof
A technology of jade and Jun porcelain, which is applied in the field of Jun porcelain jade glaze and its preparation, can solve the problems of reducing the value of jade glaze, low success rate of coal firing, old color of Jun porcelain, etc., and achieves widening firing range, strong jade texture, The effect of enhancing gloss
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] A Jun porcelain jade glaze, characterized in that it is prepared from the following raw materials in parts by weight: 52-58 parts of feldspar, 19-25 parts of quartz, 13-19 parts of calcite, 1.5-2.5 parts of talc, 2.5 parts of zinc oxide -3.5 parts, 0.5-1.5 parts of tin oxide, 0.25-0.75 parts of copper oxide.
[0025] The preparation method of above-mentioned Jun porcelain jade glaze, comprises the following steps:
[0026] (1) Preparation of glaze slurry: Add appropriate amount of water to mix the above raw materials, and ball mill to obtain glaze slurry with a mass concentration of 52-54%;
[0027] (2) Glazing: immerse the green body in the glaze slurry prepared in step (1) for a while, then immerse it again for a while, take it out, use the water absorption of the green body to make the glaze slurry adhere to the surface of the green body, then dry, and then brush 2-3 times of glaze slurry, so that the thickness of the glaze layer is 1.2-1.5mm;
[0028] (3) Firing, ...
Embodiment 2
[0036] A Jun porcelain jade glaze is prepared from the following raw materials in parts by weight: 55 parts of feldspar, 22 parts of quartz, 16 parts of calcite, 2 parts of talc, 3 parts of zinc oxide, 1 part of tin oxide and 0.5 part of copper oxide.
[0037] The preparation method of above-mentioned Jun porcelain jade glaze, comprises the following steps:
[0038] (1) Preparation of glaze slurry: Add appropriate amount of water to mix the above raw materials, and ball mill to obtain a glaze slurry with a mass concentration of 53%;
[0039] (2) Glazing: immerse the green body in the glaze slurry prepared in step (1) for a while, then immerse it again for a while, take it out, use the water absorption of the green body to make the glaze slurry adhere to the surface of the green body, then dry, and then brush 2-3 times of glaze slurry, so that the thickness of the glaze layer is 1.25mm;
[0040] (3) Firing, the firing temperature is 1310°C;
[0041] The firing process specifi...
Embodiment 3
[0048] A Jun porcelain jade glaze is prepared from the following raw materials in parts by weight: 52 parts of feldspar, 25 parts of quartz, 14 parts of calcite, 2 parts of talc, 3.5 parts of zinc oxide, 0.9 part of tin oxide and 0.4 part of copper oxide.
[0049] The preparation method of above-mentioned Jun porcelain jade glaze, comprises the following steps:
[0050] (1) Preparation of glaze slurry: Add appropriate amount of water to mix the above raw materials, and ball mill to obtain a glaze slurry with a mass concentration of 54%;
[0051] (2) Glazing: immerse the green body in the glaze slurry prepared in step (1) for a while, then immerse it again for a while, take it out, use the water absorption of the green body to make the glaze slurry adhere to the surface of the green body, then dry, and then brush 2-3 times of glaze slurry, so that the thickness of the glaze layer is 1.5mm;
[0052] (3) Firing, the firing temperature is 1320°C;
[0053] The firing process spec...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com