Wood processing technology for manufacturing seamless antique furniture
A kind of wood treatment and wood technology, applied in wood treatment, pressurized wood treatment, wood treatment details, etc., can solve the problems of looseness, shrinkage, expansion, unfavorable handing down for centuries, etc., and achieve the effect of prolonging life, saving maintenance and prolonging life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] Take rosewood as an example
[0020] It includes the following steps:
[0021] ①Compression and shaping: First, the rosewood wood is steamed and treated at a high temperature of 120℃-180℃ for 24 hours; the wood fiber is expanded and softened, and then the wood is placed on a water vapor heating platform of 120℃-180℃ for high temperature, pressure, and shaping. The thickness is 45mm, processing for 8 hours;
[0022] ②High-temperature wax injection: the shaped wood is waxed at a high temperature of 80℃-100℃, and the water molecules are replaced with wax molecules for continuous treatment for 7-15 days; then the wood is placed on a water vapor heating platform at 120℃-180℃, Carry out high temperature, pressurization and shaping on the waxed wood for 8 hours;
[0023] ③Professional isolation glue sealing: The isolation glue is closed for five consecutive times.
Embodiment 2
[0025] Take chicken wing wood as an example
[0026] It includes the following steps:
[0027] ①Compression and shaping: First, the chicken wing wood is cooked at a high temperature of 120°C-180°C for 24 hours; the wood fiber is expanded and softened, and then the wood is placed on a water vapor heating platform at 120°C-180°C for high temperature, pressure, and shaping. The thickness is 38mm, processing for 3 hours;
[0028] ②High-temperature wax injection: the shaped wood is waxed at a high temperature of 80℃-100℃, and the water molecules are replaced with wax molecules for continuous treatment for 7-15 days; then the wood is placed on a water vapor heating platform at 120℃-180℃, Carry out high temperature, pressurization and shaping on the waxed wood for 3 hours;
[0029] ③Professional isolation glue sealing: The isolation glue is closed for five consecutive times.
Embodiment 3
[0031] Take rosewood as an example
[0032] It includes the following steps:
[0033] ①Compression and shaping: First, the rosewood wood is cooked at a high temperature of 120°C-180°C for 24 hours; the wood fiber is expanded and softened, and then the wood is placed on a steam heating platform at 120°C-180°C to perform high temperature, pressurization, shaping, and thickness 47mm, processing for 8 hours;
[0034] ②High-temperature wax injection: the shaped wood is waxed at a high temperature of 80℃-100℃, and the water molecules are replaced with wax molecules for continuous treatment for 7-15 days; then the wood is placed on a water vapor heating platform at 120℃-180℃, Carry out high temperature, pressurization and shaping on the waxed wood for 8 hours;
[0035] ③Professional isolation glue sealing: The isolation glue is closed for five consecutive times.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com